A method for preparing oil-soluble amorphous nickel-boron alloy
An amorphous nickel-boron alloy was generated by reacting nickel acetate, sodium hydroxide, and sodium borohydride, and then surface-modified with polyvinylpyrrolidone and 4103A. This solved the problem of easy agglomeration of metal nanoparticles and achieved good dispersibility and anti-wear properties in lubricating oil.
Patent Information
- Application Number
- CN202211301265.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Metal nanoparticles are prone to agglomeration, which leads to larger particle sizes and limits their application in lubricating oils.
Amorphous nickel-boron alloys are generated by reacting nickel acetate, sodium hydroxide, and sodium borohydride, and then surface-modified with polyvinylpyrrolidone and a high-molecular-weight block polymer containing acidic groups, such as 4103A, to form oil-soluble amorphous nickel-boron alloys.
The dispersibility and anti-wear properties of amorphous nickel-boron alloys in lubricating oil were improved, and long-term stable dispersion was achieved through the synergistic effect of PVP and 4103A.
Smart Images

Figure CN115870492B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of amorphous alloy materials, and in particular to a method for preparing an oil-soluble amorphous nickel-boron alloy. Background Art
[0002] Nano-metal materials have many properties and are widely used in catalysts, lubricant additives, magnetic powders, structural enhancers of polymer materials, thermal conductive pastes and conductive inks. Among them, the application of nano-metal particles in lubricants has received extensive attention. Nano-copper and nano-nickel have significantly improved the friction and wear properties of lubricants, and amorphous Ni-B alloy particles also have anti-wear and friction-reducing properties.
[0003] Patent announcement CN112852522A in the prior art discloses a block type poly (methyl) acrylate polymer as a nano copper additive in lubricating oil, which can make nano copper dispersed well in oil. The invention uses a variety of active groups to disperse amorphous Ni-B alloy, prepares an amorphous nano particle dispersion system with good oil solubility, and applies it to the anti-wear and friction reducing additive of lubricating oil. Patent document CN108559580A discloses a nano alloy containing copper, nickel and titanium, which is developed into an energy-saving soft alloy atomic oil film lubricating oil additive with good lubrication properties. Patent document CN101612667 discloses a method of preparing oil-soluble nano copper using alkyl phosphonic acid, alkyl thiophosphoric acid, alkyl hydroxamic acid, alkyl salicylaldehyde oxime and the like as modifiers.
[0004] However, metal nanoparticles have a large specific surface area and high surface activity. Unmodified nanometal particles are prone to agglomeration and form secondary particles, which increases the particle size of the nanoparticles and produces precipitation, thus limiting the application of nanoparticles. Although nanoparticles can be dispersed in liquid media well by strong stirring or ultrasound, once the stirring or ultrasound is stopped, the particles will aggregate with each other due to the intermolecular force. In order to change this situation, chemical methods are used to change the surface properties of the particles, change the interaction between the particles and the liquid medium, and between the particles, and enhance the repulsive force between the particles, which will produce a lasting effect of inhibiting flocculation and agglomeration. Summary of the invention
[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing an oil-soluble amorphous nickel-boron alloy, which adopts a combination of new components, ratios and processes to solve the above technical problems.
[0006] The purpose of the present invention is achieved by the following technical solutions:
[0007] A method for preparing an oil-soluble amorphous nickel-boron alloy comprises the following steps:
[0008] S1: adding nickel salt to ultrapure water, stirring the nickel salt to completely dissolve, to obtain solution A; adding sodium hydroxide to ultrapure water to prepare a sodium hydroxide solution, and then adding sodium borohydride to the sodium hydroxide solution to obtain solution B;
[0009] S2: Place solution A in a three-necked flask in a constant temperature water bath, transfer solution B to a constant pressure funnel and slowly add it dropwise to solution A, continue the reaction after the titration is completed, obtain a solid product through centrifugation and washing, and then vacuum dry the product to obtain an amorphous nickel-boron alloy;
[0010] S3: The prepared amorphous nickel-boron alloy is surface-modified with a high molecular block polymer containing an acidic group to obtain an oil-soluble amorphous nickel-boron alloy.
[0011] Preferably, in step S1, the nickel salt includes at least one of nickel sulfate, nickel acetate and nickel chloride.
[0012] More preferably, in step S1, the nickel salt is nickel acetate.
[0013] Preferably, in step S1, the molar ratio of nickel salt to sodium borohydride is 1:(1-5).
[0014] More preferably, in step S1, the molar ratio of nickel salt to sodium borohydride is preferably 1:3.
[0015] Preferably, in step S1, in solution B, the molar ratio of sodium hydroxide to sodium borohydride is preferably 1:2.
[0016] Preferably, in step S1, the concentration of nickel salt is 0.2 mol / L, the concentration of sodium hydroxide is 0.2 mol / L, and the concentration of sodium borohydride is 0.4 mol / L.
[0017] Preferably, in step S2, polyvinyl pyrrolidone (PVP) is added to solution A, stirred to dissolve the PVP, solution B is transferred to a constant pressure funnel, and solution B is slowly added dropwise to solution A.
[0018] Preferably, in step S2, the mass ratio of nickel to polyvinyl pyrrolidone is 1:(0-4).
[0019] More preferably, in step S2, the mass ratio of the metal Ni ions to the mass ratio of the polyvinyl pyrrolidone is preferably 1:2.
[0020] Preferably, in step S2, the reaction temperature is an ice bath and the reaction time is 1 h.
[0021] Preferably, in step S2, solution B is added dropwise slowly, i.e., at 3.5 mL / min.
[0022] Preferably, in step S2, washing is performed with ultrapure water and ethanol, and the number of washing times is 6 times.
[0023] Preferably, in step S2, the centrifugal speed is 8000 rpm and the centrifugal time is 5 min.
[0024] Preferably, in step S2, the vacuum drying temperature is 60°C, and the vacuum drying time is 12h to 24h.
[0025] Preferably, in step S3, the high molecular block polymer containing an acidic group is a dispersant comprising a reaction product of a phosphorylating agent (such as polyphosphoric acid) and an R-OH compound, wherein R is a residue of a polyester or polyether having a polymerization end group, and wherein the molar ratio of the phosphorus atom in the phosphorylating agent to R-OH is (1.3 to 3):1; the dispersant is considered to be a pyrophosphate ester (4103A anti-settling dispersant).
[0026] Preferably, in step S3, when the surface is modified with a high molecular block polymer (4103A) containing an acidic group, it needs to be added to the base oil before the dispersion performance test, and the high molecular block polymer (4103A) containing an acidic group accounts for 1.5%-3.5% of the base oil mass.
[0027] Preferably, in step S3, the mass ratio of the amorphous nickel-boron alloy to the base oil is (0.5-2.5):(97.5-99.5).
[0028] The beneficial effects of the present invention are:
[0029] The method provided by the present invention adopts a combination of new components, ratios and processes, so that the prepared amorphous nickel-boron alloy has good dispersibility in lubricating oil and good anti-wear performance, and its use as a dispersant for nickel-boron alloy has not been reported. The amorphous nickel-boron alloy prepared by the present invention is added with two dispersants, PVP and 4103A, during the preparation process. It can be seen from the experimental comparison of the present invention that the two dispersants, PVP and 4103A, have a synergistic effect on improving the dispersibility of the amorphous nickel-boron alloy in 150N base oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0031] Figure 1 It is a comparison chart of the dispersibility of amorphous nickel-boron alloy with and without PVP in 150N base oil of Example 1-2.
[0032] Figure 2 It is a comparison chart of the dispersibility of amorphous nickel-boron alloy in 150N base oil between Examples 1 and 6 and Comparative Examples 1-2 with and without the high molecular block polymer (4103A) containing acidic groups.
[0033] Figure 3 It is a comparison chart of the effects of different addition amounts of high molecular block polymer (4103A) containing acidic groups in Examples 1-4 on the sedimentation ratio of amorphous nickel-boron alloy in 150N base oil. DETAILED DESCRIPTION
[0034] In order to more clearly illustrate the present invention and have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0035] The present invention adopts a chemical dispersion method to disperse metal nanoparticles. Its essence is to change the surface structure and properties of nanometal by adding a surface dispersant to achieve the effect of solubilization. The present invention is aimed at the needs of super dispersant dispersion and mixed dispersant synergistic dispersion of nanomaterials, and utilizes the synergistic effect between the groups contained in the dispersant and between different dispersants to achieve effective control of slurry agglomeration. Super dispersant dispersion overcomes the limitations of traditional dispersants in non-aqueous systems. Compared with traditional dispersants, it can form multi-point anchoring on the particle surface, improves the adsorption firmness, and is not easy to be resolved.
[0036] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0037] The present invention is further described in conjunction with the following examples.
[0038] Example 1
[0039] See attached Figure 1-3 The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment specifically comprises the following steps:
[0040] The preparation method of an amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and 4103A and PVP added comprises the following steps:
[0041] (1) 0.01 mol of nickel acetate and 50 ml of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0042] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0043] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0044] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0045] (5) Weigh a certain mass of 150N base oil, then weigh 2.5% of the mass fraction of 150N base oil of a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil of an amorphous nickel-boron alloy and add it to the 150N base oil, stir magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0046] Example 2
[0047] The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment, based on the embodiment 1, further comprises the following steps:
[0048] The preparation method of the amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and the addition of 4103A and PVP comprises the following steps:
[0049] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0050] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0051] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0052] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0053] (5) Weigh a certain mass of 150N base oil, then weigh 1.5% of the mass fraction of 150N base oil of a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil of an amorphous nickel-boron alloy and add it to the 150N base oil, stir magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0054] Example 3
[0055] The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment, based on embodiments 1 and 2, further comprises the following steps:
[0056] The preparation method of an amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and 4103A and PVP added comprises the following steps:
[0057] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0058] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0059] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0060] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0061] (5) Weigh a certain mass of 150N base oil, then weigh 2% of the mass fraction of 150N base oil and a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir it magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil and add it to the 150N base oil. Stir it magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0062] Example 4
[0063] The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment, based on embodiments 1-3, further comprises the following steps:
[0064] The preparation method of an amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and 4103A and PVP added comprises the following steps:
[0065] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0066] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0067] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0068] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0069] (5) Weigh a certain mass of 150N base oil, then weigh 3.0% of the mass fraction of 150N base oil of a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil of an amorphous nickel-boron alloy and add it to the 150N base oil, stir magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0070] Example 5
[0071] The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment, based on embodiments 1-4, further comprises the following steps:
[0072] The preparation method of an amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and 4103A and PVP added comprises the following steps:
[0073] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0074] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0075] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0076] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0077] (5) Weigh a certain mass of 150N base oil, then weigh 3.5% of the mass fraction of 150N base oil of a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil of an amorphous nickel-boron alloy and add it to the 150N base oil, stir magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0078] Example 6
[0079] The method for preparing the dispersible amorphous nickel-boron alloy provided in this embodiment, based on embodiments 1-5, further comprises the following steps:
[0080] A method for preparing an amorphous nickel-boron alloy having a molar ratio of Ni:B of 1:3 and adding 4103A but not adding PVP comprises the following steps:
[0081] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0082] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0083] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0084] (4) The product was centrifugally washed three times with ultrapure water and anhydrous ethanol at a rotation speed of 8000 rpm for 5 min, and the solid product was vacuum dried at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3.
[0085] (5) Weigh a certain mass of 150N base oil, then weigh 2.5% of the mass fraction of 150N base oil of a high molecular block polymer (4103A) containing acidic groups and add it to the 150N base oil, and stir magnetically for one hour to make it evenly dispersed in the 150N base oil. After stirring, weigh 0.5% of the mass fraction of 150N base oil of an amorphous nickel-boron alloy and add it to the 150N base oil, stir magnetically at room temperature for 0.5h, and then perform ultrasound. After ultrasound for 1h, transfer it to a test tube with a scale for storage and observe its sedimentation.
[0086] Comparative Example 1
[0087] The preparation method of the dispersible amorphous nickel-boron alloy provided in this comparative example comprises the following steps:
[0088] The preparation method of an amorphous nickel-boron alloy with a molar ratio of Ni:B of 1:3 and PVP added comprises the following steps:
[0089] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, placed in an ice bath and stirred to completely dissolve the nickel acetate, and then added to form a nickel acetate solution (solution A).
[0090] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0091] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, magnetic stirring was performed under ice bath for 1 h until the reaction was complete.
[0092] (4) washing the product by centrifugation three times with ultrapure water and anhydrous ethanol respectively at a rotation speed of 8000 rpm for 5 min, taking the solid product and vacuum drying it at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3;
[0093] (5) Weigh 10 g of 150 N base oil, then weigh an amorphous nickel-boron alloy with a mass fraction of 0.5% of the base oil mass and add it to the 150 N base oil. Stir magnetically at room temperature for 0.5 h, then perform ultrasound. After ultrasound for 1 h, transfer the alloy to a graduated test tube for storage, and observe its sedimentation.
[0094] Comparative Example 2
[0095] The preparation method of the dispersible amorphous nickel-boron alloy provided in this comparative example is specifically as follows:
[0096] A method for preparing an amorphous nickel-boron alloy having a molar ratio of Ni:B of 1:3 and without adding PVP comprises the following steps:
[0097] (1) 0.01 mol of nickel acetate and 50 mL of ultrapure water were placed in a three-necked flask, which was placed in an ice bath and stirred to completely dissolve the nickel acetate, thereby forming a nickel acetate solution (solution A).
[0098] (2) 0.015 mol of sodium hydroxide was dissolved in 75 mL of ultrapure water, and then 0.03 mol of sodium borohydride was added to form a mixed solution of sodium hydroxide and sodium hydroxide (solution B).
[0099] (3) Solution B was slowly added dropwise to solution A. After the titration was completed, the mixture was magnetically stirred in an ice bath for 1 h. The reaction was complete.
[0100] (4) washing the product by centrifugation three times with ultrapure water and anhydrous ethanol respectively at a rotation speed of 8000 rpm for 5 min, taking the solid product and vacuum drying it at 60° C. for 12 h to obtain an amorphous nickel-boron alloy with a Ni:B molar ratio of 1:3;
[0101] (5) Weigh a certain mass of 150N base oil, then weigh an amorphous nickel-boron alloy with a mass fraction of 0.5% of the base oil mass and add it to the 150N base oil. Stir magnetically at room temperature for 0.5 h, then perform ultrasound. After ultrasound for 1 h, transfer the alloy to a graduated test tube for storage, and observe its sedimentation.
[0102] Specific comparison and verification:
[0103] The comparison of the effect of PVP on the dispersibility of amorphous nickel-boron alloy in Comparative Examples 1-2 is shown in Figure 1 As shown. Figure 1It can be seen that when just dispersed, whether PVP is added or not, it can be evenly dispersed in 150N base oil; after 5 hours, the one without PVP has begun to settle, while the one with PVP can still be evenly dispersed; after one day, the one without PVP has completely settled, and the one with PVP also began to settle, but the dispersibility is still better than that without PVP, and after two days, whether PVP is added or not, it has completely settled. So it can be known that the presence or absence of PVP has a certain effect on the dispersibility of amorphous nickel-boron alloy in 150N base oil, but simply adding PVP has little effect on improving dispersibility.
[0104] Examples 1 and 6 and Comparative Examples 1-2 are comparisons of the effects of using a high molecular weight block polymer (4103A) containing an acidic group as a dispersant on dispersibility. Figure 2 As shown. Figure 2 It can be seen that 4103A is effective in improving the dispersibility. If amorphous nickel-boron is added with 4103A without PVP, a part of it will settle after one day, and on the third day it will be the same as the state without PVP. However, the dispersibility of the one with both PVP and 4103A is very good, and there is only a little stratification on the third day. Therefore, it can be seen that PVP and 4103A have a synergistic effect on improving the dispersibility of amorphous nickel-boron alloy in 150N base oil.
[0105] Examples 1-5 are comparisons of the effect of the amount of high molecular weight block polymer (4103A) containing acidic groups as a dispersant on the dispersibility. Figure 3 As shown, from Figure 3 It can be seen that the dispersibility of different 4103A addition amounts is similar on the first day; through observation of the samples for 21 days, it can be known that the sedimentation ratios of 4103A addition amounts of 2wt%, 2.5wt%, 3wt%, and 3.5wt% after 21 days are basically the same, and when the addition amount of 4103A is 1.5wt%, the sedimentation phenomenon is the most serious within 21 days, but when the addition amount of 4103A is 2.5%, the sedimentation ratio is the lowest. Therefore, when the addition amount of 4103A is 2.5wt%, the amorphous nickel-boron alloy has the best dispersibility in 150N base oil.
[0106] The preparation method provided by the above embodiment of the present invention adopts a combination of new components, ratios and processes, so that the prepared amorphous nickel-boron alloy has good dispersibility in lubricating oil and good anti-wear performance, and its use as a dispersant for nickel-boron alloy has not been reported. The amorphous nickel-boron alloy prepared by the present invention is added with two dispersants, PVP and 4103A, during the preparation process. It can be seen from the experimental comparison of the present invention that the two dispersants, PVP and 4103A, have a synergistic effect on improving the dispersibility of the amorphous nickel-boron alloy in 150N base oil.
[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing an oil-soluble amorphous nickel-boron alloy, characterized in that: The following steps are involved: S1: Add nickel salt into ultrapure water, stir and completely dissolve the nickel salt to obtain solution A; Adding sodium hydroxide into ultrapure water to prepare a sodium hydroxide solution, and then adding sodium borohydride into the sodium hydroxide solution to obtain a B solution; S2: Place solution A in a three-necked flask in a constant temperature water bath, transfer solution B to a constant pressure funnel and slowly add it dropwise to solution A, continue the reaction after the titration is completed, obtain a solid product through centrifugation and washing, and then vacuum dry the product to obtain an amorphous nickel-boron alloy; S3: surface-modifying the prepared amorphous nickel-boron alloy with a high molecular block polymer containing an acidic group, thereby obtaining an oil-soluble amorphous nickel-boron alloy; In step S1, the nickel salt includes at least one of nickel sulfate, nickel acetate, and nickel chloride; In step S1, the molar ratio of nickel salt to sodium borohydride is 1:(1-5); In step S2, polyvinyl pyrrolidone (PVP) is added to solution A, stirred to dissolve the PVP, solution B is transferred to a constant pressure funnel, and solution B is slowly added dropwise to solution A; the mass ratio of nickel to polyvinyl pyrrolidone is 1:(0-4); In step S3, the high molecular block polymer containing an acidic group is a pyrophosphate comprising a reaction product of a phosphorylating agent and an R-OH compound, wherein R is a residue of a polyester or polyether having a polymerization terminal group, and wherein the molar ratio of the phosphorus atom in the phosphorylating agent to the R-OH is (1.3 to 3):
1.
2. The method for preparing an oil-soluble amorphous nickel-boron alloy according to claim 1, characterized in that: In step S1, in solution B, the molar ratio of sodium hydroxide to sodium borohydride is 1:
2.
3. The method for preparing an oil-soluble amorphous nickel-boron alloy according to claim 1, characterized in that: In step S2, the reaction temperature is an ice bath and the reaction time is 1 h.
4. The method for preparing an oil-soluble amorphous nickel-boron alloy according to claim 1, characterized in that: In step S2, the B solution is added dropwise slowly, i.e., at 3.5 mL / min.
5. The method for preparing an oil-soluble amorphous nickel-boron alloy according to claim 1, characterized in that: In step S2, washing is performed with ultrapure water and ethanol for 6 times; the centrifugal speed is 8000 rpm, and the centrifugal time is 5 min; the vacuum drying temperature is 60° C., and the vacuum drying time is 12 h to 24 h.
6. The method for preparing an oil-soluble amorphous nickel-boron alloy according to claim 1, characterized in that: In step S3, when the surface is modified with a high molecular block polymer containing an acidic group, it needs to be added to the base oil before the dispersion performance test, and the high molecular block polymer containing an acidic group accounts for 1.5%-3.5% of the base oil mass; the mass ratio of the amorphous nickel-boron alloy to the base oil is (0.5-2.5): (97.5-99.5).