A high-aluminum cored wire for ferrite ductile iron and a preparation method thereof

By preparing high-alumina cored wire, the problems of inaccurate control of Al content and severe oxidation in ferritic ductile iron were solved, thereby improving the high strength, toughness and fatigue performance of the castings and meeting the service requirements under high fatigue environment.

CN115874015BActive Publication Date: 2024-11-12YUZHOU HENGLILAI ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211641825.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-11-12
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

In the current production of ferritic ductile iron, the Al content is not accurately controlled, resulting in severe oxidation and unstable casting quality, making it difficult to meet the requirements for high fatigue performance.

Method used

High-alumina cored wire, containing components such as Mg, Re, Ca, Al, Si, and Ti, is produced through smelting, casting, crushing, sieving, and winding processes. This ensures accurate Al content and reduces oxidation, meeting the production requirements of ferritic ductile iron.

Benefits of technology

It achieves precise control of Al content, improves the strength and toughness of castings, reduces oxidation loss, and has a simple and environmentally friendly production process that meets industry standards, thereby enhancing the quality reliability and long fatigue service life of castings.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-aluminum cored wire for ferritic ductile iron and a preparation method thereof, and relates to the technical field of cored wires. The mass percentages of the components in the high-aluminum cored wire of the invention are as follows: Mg 24% to 30%, Re 2.5 to 3.5%, Ca 2.5 to 3.5%, Al 15 to 17%, Si 0 to 30%, Ti 0 to 0.3%, and the rest are Fe and inevitable impurities. The use of the cored wire of the invention to produce ferritic ductile iron parts can effectively solve the problems of high strength, low toughness, difficult to control Al content, severe oxidation, etc. in the production of existing ferritic ductile iron parts, and at the same time make the production of ferritic ductile iron simple to operate, high alloy utilization (less oxidation), and easy to control the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cored wires, and in particular relates to a high-aluminum cored wire for ferrite ductile iron and a preparation method thereof. Background Art

[0002] Ferritic ductile iron has good plasticity and low strength, and meets the service performance requirements of glass molds under low load and high fatigue life. The traditional preparation method of ferritic ductile iron is generally obtained by increasing the Si content in cast iron and combining it with graphitization annealing. The high Si content in cast iron will increase the strength of cast iron due to the obvious solid solution strengthening effect of Si on Fe, thereby reducing the plasticity and fatigue properties of cast iron. Therefore, ferritic ductile iron with high Si content is not an ideal preparation material for high fatigue life castings. Compared with Si, Al has a stronger ability to promote the graphitization of C during the solidification of cast iron, which is more conducive to the precipitation of C in cast iron in the form of graphite, thereby making cast iron more conducive to obtaining ferrite matrix cast iron; at the same time, compared with Si, Al has a much smaller solid solution strengthening effect on Fe, so the adverse effect of Al solid solution in Fe on the fatigue properties of cast iron is much smaller than the adverse effect of Si solid solution in Fe on the fatigue properties of castings. Therefore, using Al to partially replace Si in cast iron for the production of ferritic ductile iron parts can not only make it easier to obtain ferrite-based ductile iron, but also improve the fatigue life and fatigue performance of ductile iron parts, which has important practical significance for the production of ferritic ductile iron parts with high fatigue performance.

[0003] The Si content of conventional ferritic ductile iron is generally 2.0-3.4% (the Si content of heat-treated ferritic ductile iron is the lower limit; the Si content of cast ferritic ductile iron is the upper limit). Therefore, the Al content of ferritic ductile iron prepared by partially replacing Si with Al is generally about 1-2%. This value belongs to a low content component in cast iron, and Al belongs to a low melting point metal. Therefore, when adding 1-2% Al to cast iron, the conventional method is generally to lay weighed Al powder together with the inoculant at the bottom of the ladle, and then use the high-temperature molten iron to melt the Al powder and the inoculant when the molten iron is poured into the ladle, so that the required Al content is obtained in the molten iron. When adding Al to cast iron by this method, since Al is easily oxidized, it causes a large amount of slag in the molten iron and inaccurate control of the Al content. Therefore, changing the method of adding low Al content to cast iron is very important for accurately controlling the Al content of the molten iron and obtaining high-quality ferritic ductile iron.

[0004] The use of cored wire to add alloying elements such as Mg, rare earth, and Ca to molten iron by wire feeding has many advantages, such as simple operation, high alloy utilization rate (less oxidation), good composition control, environmental protection, and high reliability of the obtained casting quality, and is widely used in the industry. However, the existing ductile iron inoculated and spheroidized cored wires basically do not contain Al (the Al content in the cored wire is less than 1%). Therefore, if 1-2% Al is to be added to molten iron by wire feeding, it is necessary to develop a new high-Al-containing cored wire and its corresponding preparation method. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a high-aluminum cored wire for ferritic ductile iron and a preparation method thereof. When the high-aluminum cored wire of the present invention is used in the production of ferritic ductile iron parts, it can provide the required Al content in the molten iron, thereby obtaining a ferritic ductile iron part of higher quality.

[0006] The present invention is achieved by adopting the following technical solutions:

[0007] A high-aluminum cored wire for ferrite ductile iron, comprising the following components in percentage by mass:

[0008] Mg 24%-30%, Re 2.5-3.5%, Ca 2.5-3.5%, Al 15-17%, Si 0-30%, Ti 0-0.3%, and the rest are Fe and inevitable impurities.

[0009] The present invention also provides a method for preparing the high-aluminum cored wire for ferrite ductile iron, comprising the following steps:

[0010] Step 1, preparing raw materials for high-aluminum cored wire; according to the chemical composition requirements of the cored wire, calculating and weighing the required magnesium ingot, aluminum ingot, silicon-calcium alloy, rare earth, and ferrosilicon raw materials;

[0011] Step 2, smelting; placing the weighed ferrosilicon, aluminum ingot and silicon-calcium alloy in a medium frequency furnace for melting, and then adding magnesium ingot and rare earth, while using CO2 as a carrier gas, spraying SF6 gas into the smelting furnace for smelting to obtain an alloy melt;

[0012] Step 3, casting into an ingot: using a water-cooled ingot mold to cast the alloy melt into an ingot to obtain a cored wire alloy ingot;

[0013] Step 4, crushing: crushing the cored wire alloy ingot with a crusher, and sieving to obtain the cored wire alloy powder;

[0014] Step 5, inspection: inspect the components in the cored wire alloy powder, and reserve them after they are qualified;

[0015] Step 6, rolling into wire; using a thin steel strip to cover the core wire alloy powder on a core wire machine to form a core wire, and then using a winding machine to roll the core wire into a roll;

[0016] Step 7: Inspect, package and store the cored wire.

[0017] Preferably, when smelting and adding magnesium ingots and rare earths in step 2 of the present invention, a magnesium alloy smelting covering agent needs to be added, and the smelting furnace power needs to be controlled so that the magnesium ingots and rare earths are quickly melted and mixed evenly, and then the temperature is quickly raised to 680-700°C.

[0018] Preferably, during casting in step 3, the distance between the medium frequency furnace mouth and the ingot mold is 200 to 400 mm.

[0019] Preferably, the crushing and screening in step 4 are carried out in a nitrogen or argon protective atmosphere to prevent oxidation of the wire core alloy during the crushing process; the particle size of the core wire alloy powder after screening is 0.1mm to 2.5mm.

[0020] Preferably, when the thin steel strip is used to coat the wire core powder in step 6, the steel strip interface is mechanically engaged.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a high-aluminum cored wire for ferrite matrix ductile iron. The cored wire of the present invention is used to produce ferrite ductile iron parts, which can effectively solve the problems of high strength, low toughness, difficult to control Al content, severe oxidation and the like in the existing production of ferrite ductile iron parts. At the same time, the ferrite ductile iron production operation is simple, the alloy utilization rate is high (less oxidation), the composition controllability is good, the environment is environmentally friendly, the quality reliability of the obtained castings is high, and many other advantages are achieved, which is of great significance to the production of ferrite ductile iron and the improvement of service life in a high fatigue service environment. At the same time, the cored wire prepared by the present invention meets the requirements of JB / T13472-2108. DETAILED DESCRIPTION

[0023] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0024] Example 1

[0025] A high-aluminum cored wire for ferrite ductile iron, comprising the following specific steps:

[0026] Step 1: Preparation of alloy powder raw materials for cored wire: Calculate and weigh the required amount of raw materials such as magnesium ingot, aluminum ingot, calcium silicon, rare earth, and ferrosilicon according to the chemical composition requirements of the cored wire; the mass percentages of the chemical components in the cored wire are as follows:

[0027] Mg 24%, Re 2.5%, Ca 2.5%, Al 15%, Si 30%, Ti 0.2%, the rest is Fe and inevitable impurities;

[0028] Step 2, smelting: melt the weighed ferrosilicon, aluminum ingots and silicon-calcium alloy in a medium frequency furnace, add magnesium ingots and rare earth after they are fully dissolved, and use CO2 as carrier gas to spray SF6 gas into the smelting furnace. The temperature of the alloy smelting out of the furnace is 680℃; the alloy melt obtained after smelting;

[0029] Step 3, casting into an ingot: using a water-cooled ingot mold to cast the alloy melt into an ingot to obtain a cored wire alloy ingot; during casting, the distance between the medium frequency furnace port and the ingot mold is 200 mm;

[0030] Step 4, crushing the cored wire alloy ingot into powder: crushing the cored wire alloy ingot with a crusher, and sieving the alloy powder with a sieving machine; the particle size of the powder after sieving is: 0.1mm ~ 2.5mm.

[0031] Step 5: Composition inspection: chemical analysis is used to inspect the composition of the cored wire powder;

[0032] Step 6, rolling into wire: using thin steel strip to cover the core wire powder on the core wire machine and make it into wire, and then using a winding machine to roll the core wire into a coil; the specifications of the core wire produced meet the requirements of JB / T13472-2108;

[0033] Step 7: Inspect, package and store the cored wire.

[0034] Example 2

[0035] A high-aluminum cored wire for ferrite ductile iron, comprising the following specific steps:

[0036] Step 1. Configuration of the core wire alloy powder raw materials: according to the chemical composition requirements of the core wire, calculate and weigh the required amounts of raw materials such as magnesium ingot, aluminum ingot, silicon calcium, rare earth, and ferrosilicon; the mass percentages of the chemical components in the core wire are as follows:

[0037] Mg 30%, Re 3.5%, Ca 3.5%, Al 20%, Si 20%, Ti 0.1%, and the remainder is Fe and inevitable impurities.

[0038] Step 2, smelting: melt the weighed ferrosilicon, aluminum ingots and silicon-calcium alloy in a medium frequency furnace, add magnesium ingots and rare earth after they are fully dissolved, and use CO2 as carrier gas to spray SF6 gas into the smelting furnace. The alloy smelting furnace temperature is 700℃; the alloy melt obtained after smelting;

[0039] Step 3, casting into an ingot: using a water-cooled ingot mold to cast the alloy melt into an ingot to obtain a cored wire alloy ingot; during casting, the distance between the intermediate frequency furnace port and the ingot mold is 400 mm;

[0040] Step 4, crushing the cored wire alloy ingot into powder: crushing the cored wire alloy ingot with a crusher, and sieving the alloy powder with a sieving machine; the particle size of the powder after sieving is: 0.1mm ~ 2.5mm.

[0041] Step 5: Composition inspection: chemical analysis is used to inspect the composition of the cored wire powder;

[0042] Step 6, rolling into wire: using thin steel strip to cover the core wire powder on the core wire machine and make it into wire, and then using a winding machine to roll the core wire into a coil; the specifications of the core wire produced meet the requirements of JB / T13472-2108;

[0043] Step 7: Inspect, package and store the cored wire.

[0044] Example 3

[0045] A high-aluminum cored wire for ferrite ductile iron, comprising the following specific steps:

[0046] Step 1: Preparation of alloy powder raw materials for cored wire: Calculate and weigh the required amount of raw materials such as magnesium ingot, aluminum ingot, calcium silicon, rare earth, and ferrosilicon according to the chemical composition requirements of the cored wire; the mass percentages of the chemical components in the cored wire are as follows:

[0047] Mg 26%, Re 3.0%, Ca 3.0%, Al 17%, Si 10%, Ti 0.1%, the rest is Fe and inevitable impurities;

[0048] Step 2, smelting: melt the weighed ferrosilicon, aluminum ingots and silicon-calcium alloy in a medium frequency furnace, add magnesium ingots and rare earth after they are fully dissolved, and use CO2 as carrier gas to spray SF6 gas into the smelting furnace. The temperature of the alloy smelting out of the furnace is 680℃; the alloy melt obtained after smelting;

[0049] Step 3, casting into an ingot: using a water-cooled ingot mold to cast the alloy melt into an ingot to obtain a cored wire alloy ingot; during casting, the distance between the intermediate frequency furnace port and the ingot mold is 300 mm;

[0050] Step 4, crushing the cored wire alloy ingot into powder: crushing the cored wire alloy ingot with a crusher, and sieving the alloy powder with a sieving machine; the particle size of the powder after sieving is: 0.1mm ~ 2.5mm.

[0051] Step 5: Composition inspection: chemical analysis is used to inspect the composition of the cored wire powder;

[0052] Step 6, rolling into wire: using thin steel strip to cover the core wire powder on the core wire machine and make it into wire, and then using a winding machine to roll the core wire into a coil; the specifications of the core wire produced meet the requirements of JB / T13472-2108;

[0053] Step 7: Inspect, package and store the cored wire.

[0054] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a high-aluminum cored wire for ferrite ductile iron, characterized in that: The following steps are involved: Step 1, preparing raw materials for high-aluminum cored wire; according to the chemical composition requirements of the cored wire, calculating and weighing the required magnesium ingot, aluminum ingot, silicon-calcium alloy, rare earth, and ferrosilicon raw materials; the core wire alloy powder of the high-aluminum cored wire includes the following components: Mg 24%~30%, RE 2.5%~3.5%, Ca 2.5%~3.5%, Al 15%~17%, Si 10%~30%, Ti 0~0.3%, the rest is Fe and inevitable impurities; Step 2, smelting; placing the weighed ferrosilicon, aluminum ingot and silicon-calcium alloy in a medium frequency furnace for melting, and then adding magnesium ingot and rare earth, while using CO2 as a carrier gas, spraying SF6 gas into the smelting furnace for smelting to obtain an alloy melt; Step 3, casting into an ingot: using a water-cooled ingot mold to cast the alloy melt into an ingot to obtain a cored wire alloy ingot; Step 4, crushing: crushing the cored wire alloy ingot with a crusher, and sieving to obtain the cored wire alloy powder; Step 5, inspection: inspect the components in the cored wire alloy powder, and reserve them after they are qualified; Step 6, rolling into wire; using a thin steel strip to cover the core wire alloy powder on a core wire machine to form a core wire, and then using a winding machine to roll the core wire into a roll; Step 7: Inspect, package and store the cored wire.

2. The preparation method according to claim 1, characterized in that: When the magnesium ingot and rare earth are added during smelting in step 2, a magnesium alloy smelting covering agent needs to be added, and the smelting furnace power needs to be controlled so that the magnesium ingot and rare earth are quickly melted and mixed evenly, and then the temperature is quickly raised to 680-700°C.

3. The preparation method according to claim 1, characterized in that: During step 3 casting, the distance between the medium frequency furnace mouth and the ingot mold is 200mm~400mm.

4. The preparation method according to claim 1, characterized in that: In step 4, the crushing and screening are carried out in a nitrogen or argon protective atmosphere to prevent oxidation of the wire core alloy during the crushing process; the particle size of the core wire alloy powder after screening is 0.1mm~2.5mm.

5. The preparation method according to claim 1, characterized in that: Step 6: When the thin steel strip is used to cover the wire core powder, the steel strip interface is mechanically engaged.