A membrane electrode and a proton exchange membrane water electrolyzer composed of the same
By using aluminum alloy reverse template in SPE electrolytic cell to prepare a surface bionic proton exchange membrane, and combining dopamine treatment to improve the binding force between the catalyst layer and the membrane, the problem of poor bonding of the catalyst layer and the proton exchange membrane is solved, and the electrolytic cell is reduced Membrane resistance and effect of improving durability.
Patent Information
- Application Number
- CN202211414730.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-11
AI Technical Summary
The existing SPE electrolytic cells have a higher resistance and poor membrane electrode activity due to poor bonding between the catalyst layer and the proton exchange membrane, and have weak durability, which limits the scale development of the device.
The surface bionic proton exchange membrane was prepared using aluminum alloy reverse template, and the adhesion between the catalyst layer and the proton exchange membrane was improved by dopamine treatment, combined with dopamine and perfluorosulfonic acid resin solution to form a catalyst slurry, and sprayed to form anode and cathode catalysts. The layer is combined with precision electrospark processing and autoclave processing to build an efficient membrane electrode.
It effectively reduces membrane resistance, improves the durability and activity of membrane electrodes, significantly reduces ohmic impedance and material transport impedance, and enables proton exchange membrane water electrolytic cell to exert high performance and long life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen production by electrolysis of water, and in particular to a membrane electrode and a proton exchange membrane water electrolyzer composed of the membrane electrode and the proton exchange membrane water electrolyzer. Background Art
[0002] Hydrogen energy is a clean, efficient and renewable energy source. Replacing fossil energy with hydrogen energy is considered an effective way to solve the energy shortage and environmental pollution problems currently faced by the world. Water electrolysis is one of the most effective technologies for preparing high-purity hydrogen. Especially in combination with renewable energy power generation technology, it can not only effectively absorb "abandoned electricity" and has good economic efficiency, but also realize a cleaner way to produce hydrogen, and has broad application prospects. Solid polymer electrolyte electrolyzers have become a new generation of water electrolysis hydrogen production devices due to their advantages such as small size, compact structure, strong pressure resistance, large working current and high hydrogen production purity. The membrane electrode is the core of the electrolyzer, which consists of a proton exchange membrane and cathode and anode catalyst coating layers on both sides. During the hydrolysis process, water generates oxygen and hydrogen ions on the anode catalyst coating side of the membrane electrode, and the hydrogen ions are reduced to generate hydrogen through the proton exchange membrane on the cathode catalyst coating layer. Therefore, the membrane electrode is a key factor affecting the hydrolysis efficiency of the electrolyzer.
[0003] At present, SPE electrolyzers are faced with problems such as poor bonding between the catalyst layer and the proton exchange membrane, resulting in increased resistance, poor activity of the membrane electrode, and weak durability, which restricts the large-scale development of SPE electrolyzers. Improving the preparation method of the membrane electrode and performing good activation treatment on the membrane electrode will make the membrane electrode conducive to building a good material transmission channel for protons, electrons, water and gas, thereby greatly reducing the ohmic impedance and material transmission impedance, which is extremely critical for the preparation of high-performance and long-lasting SPE electrolyzers. However, how to study the preparation and activation of suitable membrane electrodes for SPE electrolyzers is worthy of attention. Summary of the invention
[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide a proton exchange membrane water electrolyzer. By adopting an aluminum alloy counter template to make the proton exchange membrane have a surface with a striped structure similar to that of foxtail grass leaves, and using dopamine for surface treatment, the adhesion between the catalyst layer and the proton exchange membrane can be improved, the membrane resistance of the electrolyzer can be effectively reduced, and the durability and activity can be improved.
[0005] To achieve the above objectives, in a first aspect, the present invention provides a proton exchange membrane water electrolyzer, comprising a membrane electrode, wherein the membrane electrode comprises a surface biomimetic proton exchange membrane and an anode catalyst layer and a cathode catalyst layer on both sides thereof.
[0006] Optionally, the preparation method of the membrane electrode comprises the following steps: (1) preparing a surface biomimetic proton exchange membrane, and treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution; (2) mixing an anode catalyst and a perfluorosulfonic acid resin solution to form an anode catalyst slurry; mixing a cathode catalyst and a perfluorosulfonic acid resin solution to form a cathode catalyst slurry; (3) spraying the cathode catalyst slurry described in step (2) on the cathode side of the proton exchange membrane, and obtaining a cathode catalyst layer after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the proton exchange membrane, and obtaining an anode catalyst layer after drying, and finally obtaining a water electrolysis membrane electrode.
[0007] Optionally, the surface of the surface biomimetic proton exchange membrane is treated with a dopamine hydrochloride solution, and the specific steps are: spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 100-110° C. for 2-4 hours to obtain a modified surface biomimetic proton exchange membrane.
[0008] Optionally, the anode catalyst is iridium oxide, RuO 2, One or a combination of Ir single substance, Ru single substance and Ru-Ir alloy.
[0009] Optionally, the cathode catalyst is one of Pt / C or platinum black.
[0010] Optionally, the concentration of the anode catalyst slurry is 25-40 wt %; the concentration of the cathode catalyst slurry is 28-46 wt %.
[0011] Optionally, the thickness of the cathode catalyst layer is 50-100 μm; the thickness of the anode catalyst layer is 50-100 μm.
[0012] Optionally, the preparation method of the surface biomimetic proton exchange membrane comprises the following steps: (1) using the electric spark precision machining technology to process the stripe structure of the bionic foxtail grass leaf on the aluminum alloy substrate to obtain an aluminum alloy template, and pouring and defoaming the polydimethylsiloxane glue to obtain a silica gel counter template after curing; (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 30-40% and a terminal -SO3Na, adding a modified reinforcing material, stirring evenly, and after passing an inert gas into the autoclave, maintaining a pressure range of 1.5-2Mpa and a temperature of 120-150°C, and keeping the temperature for 2-10 hours, Then naturally cool to obtain a perfluorosulfonic acid resin solution doped with a modified reinforcing material; the weight volume ratio of the modified reinforcing material to the perfluorosulfonic acid resin aqueous solution with -SO3Na at the end is 15-20 g / L; the solvent of the perfluorosulfonic acid resin solution consists of water and ethanol, with a mass ratio of 20:30; (3) coating the perfluorosulfonic acid resin solution described in step (2) on the surface of the aluminum alloy reverse template described in step (1), heating to a temperature of 100-120°C, drying for 1-2 hours, and separating from the mold after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 50-100 μm.
[0013] Optionally, the modified reinforcing material is montmorillonite modified by tetrabutylammonium and dopamine intercalation or two-dimensional layered functionalized Mxene nanosheets modified by tetrabutylammonium and dopamine intercalation.
[0014] Optionally, it also includes an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode includes, from the inside to the outside, an anode gas diffusion layer, an anode guide plate and a cathode insulating plate, and the cathode side of the membrane electrode includes, from the inside to the outside, a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate; the positive and negative poles of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is for introducing deionized water into the anode side of the electrolytic cell; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper.
[0015] In order to achieve the above object, in a second aspect, the present invention provides an electrode activation method for a proton exchange membrane water electrolyzer, comprising the following steps:
[0016] (1) introducing deionized water at 90° C. at a flow rate of 200 mL / min into the anode side of the electrolytic cell;
[0017] (2) Applying a load to the electrolytic cell, first running 5 working steps in constant current mode, with the current density increasing from 0 to 5 A / cm 2 , respectively 2A / cm 2 Run for 15min at current density; 3A / cm 2 Run for 15min at current density; 4A / cm 2 Run for 20 min at current density; 5A / cm 2Run for 30 min at current density; 3.6A / cm 2 Run at the current density for 30 min;
[0018] (3) Then, three working steps were performed in the constant voltage mode, with the voltage dropping from 2 V to 1.6 V, namely, 10 min at 2 V, 10 min at 1.8 V, and 10 min at 1.6 V.
[0019] (4) Finally, switch to constant current mode, 1.5A / cm 2 Run at the current density for 30 min;
[0020] (5) After the activation step is completed, remove the load and let it sit for about 10 minutes for performance testing.
[0021] The beneficial effects of the present invention are as follows:
[0022] (1) The present invention prepares a proton exchange membrane with a striped structure similar to that of foxtail grass leaves, and then treats it with dopamine. It is found that the wettability of the catalyst slurry on its surface can be improved. The dried catalyst layer has good bonding force, which effectively reduces membrane resistance and improves durability and activity.
[0023] (2) The activation method of the present invention is directed to the proton exchange membrane water electrolyzer composed of the above-mentioned membrane electrode, and can construct the transmission channels of protons, electrons, water and gas to a large extent, reduce the ohmic impedance and material transmission impedance, and enable the proton exchange membrane water electrolyzer to exert the best performance. DETAILED DESCRIPTION
[0024] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.
[0025] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0026] First, the proton exchange membrane water electrolyzer according to the first aspect of the present invention is described. The proton exchange membrane water electrolyzer comprises a membrane electrode, which comprises a surface biomimetic proton exchange membrane and an anode catalyst layer and a cathode catalyst layer on both sides thereof.
[0027] The preparation method of the membrane electrode comprises the following steps: (1) preparing a surface biomimetic proton exchange membrane, and treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution; (2) mixing an anode catalyst and a perfluorosulfonic acid resin solution to form an anode catalyst slurry; and mixing a cathode catalyst and a perfluorosulfonic acid resin solution to form a cathode catalyst slurry; (3) spraying the cathode catalyst slurry described in step (2) on the cathode side of the proton exchange membrane, and obtaining a cathode catalyst layer after drying; and spraying the anode catalyst slurry described in step (2) on the anode side of the proton exchange membrane, and obtaining an anode catalyst layer after drying, thereby finally obtaining a water electrolysis membrane electrode.
[0028] The surface of the surface biomimetic proton exchange membrane is treated with a dopamine hydrochloride solution, and the specific steps are: spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 100-110° C. for 2-4 hours to obtain a modified surface biomimetic proton exchange membrane.
[0029] The anode catalyst is one or a combination of iridium oxide, RuO2, Ir single substance, Ru single substance and Ru-Ir alloy. The cathode catalyst is one of Pt / C or platinum black. The concentration of the anode catalyst slurry is 25-40wt%; the concentration of the cathode catalyst slurry is 28-46wt%. The thickness of the cathode catalyst layer is 50-100μm; the thickness of the anode catalyst layer is 50-100μm.
[0030] The preparation method of the surface biomimetic proton exchange membrane comprises the following steps: (1) using the electric spark precision machining technology to process the stripe structure of the bionic foxtail grass leaf on the aluminum alloy substrate to obtain the aluminum alloy template, and pouring and defoaming the polydimethylsiloxane glue to obtain the silica gel reverse template after curing; (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 30-40% and a terminal -SO3Na, adding the modified reinforcing material, stirring evenly, introducing an inert gas into the autoclave, maintaining the pressure range of 1.5-2Mpa and the temperature of 120-150°C, keeping the temperature for 2-10 hours, and then The method comprises the following steps: naturally cooling the modified reinforcing material to obtain a perfluorosulfonic acid resin solution doped with a modified reinforcing material; the weight volume ratio of the modified reinforcing material to the perfluorosulfonic acid resin aqueous solution with -SO3Na at the end is 15-20 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30; (3) coating the perfluorosulfonic acid resin solution described in step (2) on the surface of the aluminum alloy reverse template described in step (1), heating to a temperature of 100-120° C., drying for 1-2 hours, and separating the mold after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 50-100 μm.
[0031] The modified reinforcing material is montmorillonite modified by tetrabutylammonium and dopamine intercalation or two-dimensional layered functionalized Mxene nanosheet modified by tetrabutylammonium and dopamine intercalation.
[0032] The proton exchange membrane water electrolyzer also includes an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode includes an anode gas diffusion layer, an anode guide plate and a cathode insulating plate from the inside to the outside, and the cathode side of the membrane electrode includes a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate from the inside to the outside; the positive and negative electrodes of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is used to pass deionized water into the anode side of the electrolyzer; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper.
[0033] The electrode activation method of the proton exchange membrane water electrolyzer according to the second aspect of the present invention comprises the following steps: (1) introducing deionized water at 90° C. and a flow rate of 200 mL / min into the anode side of the electrolyzer; (2) applying a load to the electrolyzer, firstly running 5 working steps in a constant current mode, with the current density increasing from 0 to 5 A / cm2, namely, running at a current density of 2 A / cm2 for 15 min; running at a current density of 3 A / cm2 for 15 min; running at a current density of 4 A / cm2 for 20 min; and running at a current density of 5 A / cm2 for 15 min. m2 current density for 30 min; run at a current density of 3.6 A / cm2 for 30 min; (3) then run 3 working steps in constant voltage mode, with the voltage dropping from 2 V to 1.6 V, namely running at 2 V for 10 min; running at 1.8 V for 10 min; running at 1.6 V for 10 min; (4) finally switch to constant current mode and run at a current density of 1.5 A / cm2 for 30 min; (5) after the activation step is completed, remove the load and let it stand for about 10 minutes for performance testing.
[0034] The membrane electrode of the present invention is described in detail below in conjunction with a specific embodiment, wherein the specific structure of the proton exchange membrane water electrolyzer composed thereof includes: a membrane electrode, an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode is sequentially an anode gas diffusion layer, an anode guide plate and a cathode insulating plate from the inside to the outside, and the cathode side of the membrane electrode is sequentially a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate from the inside to the outside; the positive and negative electrodes of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is for passing deionized water into the anode side of the electrolyzer; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper. Except for the membrane electrode, the specific models of the above structure are available on the market, and the electrolyzer is assembled by oneself.
[0035] Example 1
[0036] 1. Preparation of surface biomimetic proton exchange membrane
[0037] (1) The stripe structure of the bionic foxtail grass leaf is processed on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue is poured, degassed, and solidified to obtain the silicone reverse template;
[0038] (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 40% and having a terminal with -SO3Na, adding tetrabutylammonium and dopamine intercalation modified two-dimensional layered functionalized Mxene nanosheets, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 2 MPa and a temperature of 150°C, keeping the temperature for 10 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with tetrabutylammonium and dopamine intercalation modified two-dimensional layered functionalized Mxene nanosheets; the weight volume ratio of the tetrabutylammonium and dopamine intercalation modified two-dimensional layered functionalized Mxene nanosheets to the perfluorosulfonic acid resin aqueous solution with -SO3Na is 20 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30;
[0039] (3) coating the perfluorosulfonic acid resin solution described in step (2) on the surface of the silica gel counter template described in step (1), heating to 120° C., drying for 2 h, and separating the template after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 50 μm.
[0040] 2. Preparation of membrane electrode
[0041] (1) treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution, spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 100° C. for 2 h to obtain a modified surface biomimetic proton exchange membrane;
[0042] (2) RuO2 and perfluorosulfonic acid resin solution are mixed to form an anode catalyst slurry with a concentration of 25 wt %; platinum black and perfluorosulfonic acid resin solution are mixed to form a cathode catalyst slurry with a concentration of 28 wt %;
[0043] (3) Spraying the cathode catalyst slurry described in step (2) on the cathode side of the modified surface biomimetic proton exchange membrane, and obtaining a cathode catalyst layer with a thickness of 50 μm after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the modified surface biomimetic proton exchange membrane, and obtaining an anode catalyst layer with a thickness of 50 μm after drying, and finally obtaining a water electrolysis membrane electrode.
[0044] Example 2
[0045] 1. Preparation of surface biomimetic proton exchange membrane
[0046] (1) The stripe structure of the bionic foxtail grass leaf is processed on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue is poured, degassed, and solidified to obtain the silicone reverse template;
[0047] (2) preparing a 30% mass concentration of a perfluorosulfonic acid resin solution with a terminal -SO3Na, adding tetrabutylammonium and dopamine intercalation-modified montmorillonite, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 1.5 MPa and a temperature of 120°C, keeping the temperature for 2 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with tetrabutylammonium and dopamine intercalation-modified montmorillonite; the weight volume ratio of the tetrabutylammonium and dopamine intercalation-modified montmorillonite to the terminal -SO3Na perfluorosulfonic acid resin aqueous solution is 15 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30;
[0048] (3) coating the perfluorosulfonic acid resin solution described in step (2) on the surface of the silica gel counter template described in step (1), heating to 100° C., drying for 1 h, and separating the template after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 100 μm.
[0049] 2. Preparation of membrane electrode
[0050] (1) treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution, spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 110° C. for 4 h to obtain a modified surface biomimetic proton exchange membrane;
[0051] (2) mixing iridium oxide and perfluorosulfonic acid resin solution to form an anode catalyst slurry with a concentration of 40 wt %; mixing Pt / C and perfluorosulfonic acid resin solution to form a cathode catalyst slurry with a concentration of 46 wt %;
[0052] (3) Spraying the cathode catalyst slurry described in step (2) on the cathode side of the modified surface biomimetic proton exchange membrane, and obtaining a cathode catalyst layer with a thickness of 100 μm after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the modified surface biomimetic proton exchange membrane, and obtaining an anode catalyst layer with a thickness of 100 μm after drying, and finally obtaining a water electrolysis membrane electrode.
[0053] Example 3
[0054] 1. Preparation of surface biomimetic proton exchange membrane
[0055] (1) The stripe structure of the bionic foxtail grass leaf is processed on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue is poured, degassed, and solidified to obtain the silicone reverse template;
[0056] (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 35% having a terminal -SO3Na, adding tetrabutylammonium and dopamine intercalation-modified montmorillonite, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 1.8 MPa and a temperature of 130°C, keeping the temperature for 6 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with tetrabutylammonium and dopamine intercalation-modified montmorillonite; the weight volume ratio of the tetrabutylammonium and dopamine intercalation-modified montmorillonite to the terminal -SO3Na perfluorosulfonic acid resin aqueous solution is 18 g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30;
[0057] (3) The perfluorosulfonic acid resin solution described in step (2) is applied to the surface of the silica gel counter template described in step (1), heated to 110° C., dried for 1.5 h, and separated from the template after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 80 μm.
[0058] 2. Preparation of membrane electrode
[0059] (1) treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution, spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 105° C. for 3 h to obtain a modified surface biomimetic proton exchange membrane;
[0060] (2) mixing iridium oxide and perfluorosulfonic acid resin solution to form an anode catalyst slurry with a concentration of 30 wt %; mixing Pt / C and perfluorosulfonic acid resin solution to form a cathode catalyst slurry with a concentration of 35 wt %;
[0061] (3) Spraying the cathode catalyst slurry described in step (2) on the cathode side of the modified surface biomimetic proton exchange membrane, and obtaining a cathode catalyst layer with a thickness of 80 μm after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the modified surface biomimetic proton exchange membrane, and obtaining an anode catalyst layer with a thickness of 80 μm after drying, and finally obtaining a water electrolysis membrane electrode.
[0062] Comparative Example 1
[0063] Compared with Example 3, the proton exchange membrane is prepared by a casting method instead of using an aluminum alloy reverse template coating imitating foxtail grass leaves, and other aspects are the same as Example 3.
[0064] Comparative Example 2
[0065] Except that dopamine hydrochloride is not used to treat the surface of the surface biomimetic proton exchange membrane, other aspects are the same as those of Example 3.
[0066] Activation of electrolytic cells
[0067] The membrane electrode obtained in the above examples and comparative examples was assembled into an electrolytic cell and activated. The specific steps are as follows:
[0068] (1) introducing deionized water at 90° C. at a flow rate of 200 mL / min into the anode side of the electrolytic cell;
[0069] (2) Applying a load to the electrolytic cell, first running 5 working steps in constant current mode, with the current density increasing from 0 to 5 A / cm 2 , respectively 2A / cm 2 Run for 15min at current density; 3A / cm 2 Run for 15min at current density; 4A / cm 2 Run for 20 min at current density; 5A / cm 2 Run for 30 min at current density; 3.6A / cm 2 Run at the current density for 30 min;
[0070] (3) Then, three working steps were performed in the constant voltage mode, with the voltage dropping from 2 V to 1.6 V, namely, 10 min at 2 V, 10 min at 1.8 V, and 10 min at 1.6 V.
[0071] (4) Finally, switch to constant current mode, 1.5A / cm 2 Run at the current density for 30 min;
[0072] (5) After the activation step is completed, remove the load and let it sit for about 10 minutes for performance testing.
[0073] Performance Testing
[0074] 1. Test the performance before and after activation, where the test conditions are as follows: the test conditions are 1.5V applied voltage frequency 0.01-10000Hz, amplitude 0.01mV, and the ohmic impedance is calculated based on the cell voltage and circuit density, so as to obtain the influence of the membrane electrode on the composed electrolytic cell.
[0075] 2. After 6 hours of hydrogen production by electrolysis, test the ohmic impedance under the above conditions.
[0076] The performance test results of the products obtained in the above examples and comparative examples are shown in Table 1 below:
[0077] Table 1
[0078] Test items Ohm resistance (before activation) Ohmic resistance (after activation) After 6 hours of electrolysis Example 1 0.143 0.121 0.122 Example 2 0.145 0.122 0.122 Example 3 0.141 0.120 0.121 Comparative Example 1 0.165 0.145 0.149 Comparative Example 2 0.156 0.138 0.145
[0079] As can be seen from Table 1, the present invention uses a surface proton exchange membrane with a stripe structure similar to that of foxtail grass leaves, and cooperates with the surface treatment of dopamine to improve the adhesion between the catalyst layer and the proton exchange membrane, which is manifested as an effective reduction in the membrane resistance of the electrolytic cell. After activation, the electrolytic cell composed of the membrane electrode of the present invention has an ohmic impedance reduction rate of more than 15%, while the comparative example is about 12%, indicating that the membrane electrode has good stability during the activation process, and the ohmic impedance of the electrolytic cell does not change much after 6 hours of electrolytic hydrogen production, indicating excellent durability.
[0080] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A proton exchange membrane water electrolyzer, characterized in that: It comprises a membrane electrode, wherein the membrane electrode comprises a surface biomimetic proton exchange membrane and an anode catalyst layer and a cathode catalyst layer on both sides thereof; The method for preparing the surface biomimetic proton exchange membrane comprises the following steps: (1) The stripe structure of the bionic foxtail grass leaf is processed on the aluminum alloy substrate by using the electric spark precision machining technology to obtain the aluminum alloy template, and the polydimethylsiloxane glue is poured, degassed, and solidified to obtain the silicone reverse template; (2) preparing a perfluorosulfonic acid resin solution with a mass concentration of 30-40% and having a terminal -SO3Na, adding a modified reinforcing material, stirring evenly, introducing an inert gas into an autoclave, maintaining a pressure range of 1.5-2Mpa and a temperature of 120-150°C, keeping the temperature for 2-10 hours, and then cooling naturally to obtain a perfluorosulfonic acid resin solution doped with a modified reinforcing material; the weight volume ratio of the modified reinforcing material to the perfluorosulfonic acid resin aqueous solution with a terminal -SO3Na is 15-20g / L; the solvent of the perfluorosulfonic acid resin solution is composed of water and ethanol, with a mass ratio of 20:30; (3) coating the perfluorosulfonic acid resin solution described in step (2) on the surface of the silica gel counter template described in step (1), heating the surface to 100-120° C., drying for 1-2 hours, and separating the surface after natural cooling to obtain a surface biomimetic proton exchange membrane with a thickness of 50-100 μm; The surface of the surface biomimetic proton exchange membrane is treated with a dopamine hydrochloride solution.
2. The proton exchange membrane water electrolyzer according to claim 1, characterized in that: The method for preparing the membrane electrode comprises the following steps: (1) preparing a surface biomimetic proton exchange membrane, and treating the surface of the surface biomimetic proton exchange membrane with a dopamine hydrochloride solution; (2) mixing the anode catalyst and the perfluorosulfonic acid resin solution to form an anode catalyst slurry; Mixing a cathode catalyst and a perfluorosulfonic acid resin solution to form a cathode catalyst slurry; (3) Spraying the cathode catalyst slurry described in step (2) on the cathode side of the proton exchange membrane, and obtaining a cathode catalyst layer after drying; spraying the anode catalyst slurry described in step (2) on the anode side of the proton exchange membrane, and obtaining an anode catalyst layer after drying, and finally obtaining a water electrolysis membrane electrode.
3. The proton exchange membrane water electrolyzer according to claim 2, characterized in that: The surface of the surface biomimetic proton exchange membrane is treated with a dopamine hydrochloride solution, and the specific steps are: spraying a 2 mg / mL dopamine hydrochloride solution onto the surface of the surface biomimetic proton exchange membrane, and drying at 100-110° C. for 2-4 hours to obtain a modified surface biomimetic proton exchange membrane.
4. The proton exchange membrane water electrolyzer according to claim 2, characterized in that: The anode catalyst is iridium oxide, RuO 2, One or a combination of Ir single substance, Ru single substance and Ru-Ir alloy.
5. The proton exchange membrane water electrolyzer according to claim 2, characterized in that: The cathode catalyst is one of Pt / C or platinum black.
6. The proton exchange membrane water electrolyzer according to claim 2, characterized in that: The concentration of the anode catalyst slurry is 25-40wt%; the concentration of the cathode catalyst slurry is 28-46wt%.
7. The proton exchange membrane water electrolyzer according to claim 2, characterized in that: The thickness of the cathode catalyst layer is 50-100 μm; the thickness of the anode catalyst layer is 50-100 μm.
8. The proton exchange membrane water electrolyzer according to claim 1, characterized in that: The modified reinforcing material is montmorillonite modified by tetrabutylammonium and dopamine intercalation or two-dimensional layered functionalized Mxene nanosheet modified by tetrabutylammonium and dopamine intercalation.
9. The proton exchange membrane water electrolyzer according to claim 1, characterized in that: It also includes an insulating plate, a guide plate, an external power supply and a water supply device; the anode side of the membrane electrode includes, from the inside to the outside, an anode gas diffusion layer, an anode guide plate and an anode insulating plate, and the cathode side of the membrane electrode includes, from the inside to the outside, a cathode gas diffusion layer, a cathode guide plate and a cathode insulating plate; the positive and negative poles of the external power supply are respectively connected to the anode guide plate and the cathode guide plate; the water supply device is used to introduce deionized water into the anode side of the electrolytic cell; the anode gas diffusion layer is a titanium mesh, and the cathode gas diffusion layer is a carbon paper.