A novel copper foil current collector and its preparation method and application in lithium metal batteries

Through the vertical Cu2S nanosheet array and Li2S interface layer of the new copper foil current collector, the problems of growth and side reaction of lithium dendrites in lithium metal batteries are solved, and ultrasmooth and dense deposition of lithium metal and improved battery performance are achieved.

CN115911397BActive Publication Date: 2024-11-19BEIHANG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211092228.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-11-19
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

The graphite negative electrode of traditional lithium-ion batteries is close to its theoretical capacity, making it difficult to further improve the energy density. The thermodynamic instability of the metal lithium negative electrode leads to uneven electroplating morphology and side reactions, affecting battery performance.

Method used

Using a new copper foil current collector, Cu2S nanosheets with vertical surface distribution are prepared by anodizing and vulcanizing to form a stable Li2S interface layer, inhibiting the growth and side reaction of lithium dendrites, and achieving uniform lithium deposition.

Benefits of technology

Significantly improve the smoothness and density of lithium metal electroplating, improve the electrochemical performance of lithium metal batteries, and achieve long-term stable circulation and high Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115911397B_ABST
    Figure CN115911397B_ABST
Patent Text Reader

Abstract

The present invention provides a novel copper foil current collector and a preparation method thereof and an application thereof in a lithium metal battery, and relates to the technical field of lithium metal batteries. The novel copper foil current collector provided by the present invention has a vertical nanosheet array distributed on the copper foil surface, which can increase the specific surface area of ​​the copper foil to an appropriate level. The stably existing nanosheet array structure alleviates the unlimited volume expansion of lithium metal while reducing the local current density, thereby achieving uniform charge distribution on the electrode surface, inhibiting the growth of lithium dendrites, and achieving ultra-dense and smooth deposition of metallic lithium, which provides a guarantee for the long-term stable cycle of lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium metal batteries, and in particular to a novel copper foil current collector and a preparation method thereof, and application thereof in lithium metal batteries. Background Art

[0002] At present, with the booming development of portable devices, electric vehicles, and smart grids, humans are forced to pursue a new generation of energy storage devices with higher energy density. The development of traditional commercial lithium-ion battery graphite anode has gradually approached its theoretical capacity (372mAh·g -1 ), there is limited room for improvement.

[0003] As the "holy grail" material for the next generation of lithium-based secondary battery anodes, lithium metal anodes have a high theoretical specific capacity (3860 mAh g -1 ) and extremely low electrode potential (-3.04Vvs standard hydrogen electrode) have attracted widespread attention, which can increase the energy density of lithium-ion batteries by 40% to 50%. However, only when the thickness of the metal lithium anode is reduced to less than 50μm can the energy density of lithium metal batteries be comparable to that of current commercial lithium-ion batteries. The preparation of ultra-thin lithium foil is still a considerable challenge for the current manufacturing industry, so it is a good choice to prepare a lithium metal anode of a certain thickness by electrochemical pre-deposition. However, due to the intrinsic thermodynamic instability of metallic lithium, it will induce uneven lithium plating morphology and uncontrollable side reactions, which will lead to the violent growth of lithium dendrites and the formation of a fragile natural solid electrolyte interphase (SEI).

[0004] As an indispensable component of the battery, the current collector plays a vital role in electron transfer and mechanical support of electrode materials. Commercial copper foil is used as a traditional negative electrode current collector because of its lithium-repellent nature and large local current density. The intrinsic defects of lithium metal plating will be infinitely magnified. Summary of the invention

[0005] The purpose of the present invention is to provide a novel copper foil current collector, a preparation method thereof and an application in a lithium metal battery. The novel copper foil current collector provided by the present invention is used for the deposition of lithium metal, which can significantly improve the deficiencies existing in the electroplating of lithium metal and obtain an ultra-smooth and dense lithium metal coating. When the novel copper foil current collector is applied to a lithium metal battery, the lithium metal battery has excellent electrochemical performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a novel copper foil current collector with vertically distributed Cu2S nanosheets on the surface.

[0008] Preferably, the Cu2S nanosheets have a thickness of 5 to 15 nm and a height of 1 to 3 μm.

[0009] Preferably, the Cu2S nanosheets are crystalline.

[0010] The present invention provides a method for preparing the novel copper foil current collector described in the above scheme, comprising the following steps:

[0011] A copper foil is placed as a working electrode in a sodium hydroxide solution and anodized under constant current conditions to vertically grow CuO nanosheets on the surface of the copper foil to obtain CuO NS@Cu foil;

[0012] The CuONS@Cu foil is sulfurized to obtain the novel copper foil current collector.

[0013] Preferably, the concentration of the sodium hydroxide solution is 0.8-1.2 mol / L.

[0014] Preferably, the current of the anodic oxidation is 0.1 to 0.3 mA·cm -2 , time is 1 to 3 hours.

[0015] Preferably, the sulfurization atmosphere is an Ar-H2S mixed atmosphere, and the volume ratio of Ar to H2S in the Ar-H2S mixed atmosphere is 8 to 12:1.

[0016] Preferably, the vulcanization temperature is 80-150° C., and the vulcanization time is 5-12 minutes.

[0017] Preferably, before placing the copper foil as a working electrode in the sodium hydroxide solution, the method also includes high-temperature annealing the copper foil; the high-temperature annealing temperature is 900-1100°C, the time is 1-3 hours, and the atmosphere is an Ar-H2 mixed atmosphere; the volume ratio of Ar and H2 in the Ar-H2 mixed atmosphere is 1:1.

[0018] The present invention provides the use of the novel copper foil current collector described in the above scheme or the novel copper foil current collector prepared by the preparation method described in the above scheme in a lithium metal battery.

[0019] The present invention provides a novel copper foil current collector with vertical Cu2S nanosheets distributed on the surface. The vertical nanosheet array distributed on the copper foil surface can increase the specific surface area of ​​the copper foil to an appropriate level. The stable nanosheet array structure alleviates the unlimited volume expansion of lithium metal while reducing the local current density, thereby achieving uniform charge distribution on the electrode surface, inhibiting the growth of lithium dendrites, and achieving ultra-smooth deposition of metallic lithium, providing a guarantee for the long-term stable cycle of lithium metal batteries.

[0020] In the initial stage of lithium metal deposition, the Cu2S nanosheets are converted into copper nanosheets covered with an ultra-thin Li2S interface layer (denoted as Li2S-CuNS@Cu foil) through an in-situ lithiation replacement reaction. The Li2S interface layer can adhere to the surface of lithium metal during the lithium electroplating process, thereby greatly suppressing the side reaction between the electrolyte and lithium metal. -5 S cm -1 ) can promote the vertical growth of metallic lithium, which is beneficial to homogenizing the lithium ion flux distribution and realizing the ultra-dense deposition of metallic lithium.

[0021] The present invention combines the vertically distributed nanosheet array with the Li2S SEI with high lithium ion conductivity, which can combine the above two advantages to achieve the effect of 1+1>2, have a positive impact on the smooth deposition of lithium metal, and realize an ultra-smooth and dense lithium deposition microstructure. -2 and 10mAh·cm -2 After the addition of lithium, their thicknesses are approximately 26.5 μm and 53.0 μm, respectively, which are close to the theoretical lithium foil thickness.

[0022] The results of the embodiment show that the lithium metal anode obtained by using the novel copper foil current collector of the present invention to deposit lithium metal can be assembled into a half-cell with a current of 1 mA·cm in an ether-based electrolyte. -2 The current density is 1 mAh cm -2 Under the conditions of 99.1%, the half-cell can be cycled stably for more than 1100 times with an ultra-high Coulombic efficiency of 99.1%. In carbonate electrolytes, the half-cell can be cycled for 300 times with a Coulombic efficiency of 98.8% (1mA·cm -2 The current density is 1 mAh cm -2 ). When matched with commercial cathodes (LiFePO4 (LFP) or NCM811), the full battery still exhibits good cycling performance under the conditions of high cathode loading, poor electrolyte and limited lithium source. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the preparation of the novel copper foil current collector of the present invention;

[0024] Figure 2 a is the constant current discharge / charge curve of the Cu2S NS@Cu foil electrode between 0.01 and 1.0 V for 5 cycles; b is the CV curve of the prepared Cu2S NS@Cu foil||Li battery;

[0025] Figure 3XRD patterns of copper foil, CuONS@Cu foil, Cu2S NS@Cu foil and Li2S-CuNS@Cu foil;

[0026] Figure 4-1 is a scanning electron microscope image of the CuO NS@Cu foil of Example 1;

[0027] Figure 4-2 for Figure 4-1 A magnified image of

[0028] Figure 4-3 TEM image of the CuO NS@Cu foil of Example 1;

[0029] Figure 4-4 This is a high-resolution transmission electron microscopy image of the CuO NS@Cu foil of Example 1;

[0030] Figure 5-1 is a scanning electron microscope image of the Cu2S NS@Cu foil of Example 1;

[0031] Figure 5-2 for Figure 5-1 A magnified image of

[0032] Figure 5-3 TEM image of the Cu2S NS@Cu foil of Example 1;

[0033] Figure 5-4 This is a high-resolution transmission electron microscopy image of the Cu2S NS@Cu foil of Example 1;

[0034] Figure 6-1 This is a scanning electron microscope image of the Li2S-CuNS@Cu foil of Application Example 1;

[0035] Figure 6-2 for Figure 6-1 A magnified image of

[0036] Figure 6-3 This is a low-temperature transmission electron microscopy image of Li2S-CuNS@Cu foil;

[0037] Figure 6-4 High-resolution low-temperature transmission electron microscopy image of Li2S-CuNS@Cu foil;

[0038] Figure 7 For the Cu2S NS@Cu foil in Application Example 1 at 1mA·cm -2 Scanning electron microscopy image of electroplating for 10 h at a current density of;

[0039] Figure 8In the figure, j and k are the Cu2S NS@Cu foil in application example 1 at 1 mA·cm -2 Scanning electron microscope cross-sectional images of Cu2S NS@Cu foil electroplated at a current density of 1 mA·cm -2 Scanning electron microscope cross-sectional and plan views of electroplating for 10 h at a current density of;

[0040] Fig. 9 This is a scanning electron microscope image of the copper foil after pretreatment in Comparative Example 1;

[0041] Fig.10 For comparative example 1, the copper foil is at 1 mA·cm -2 Scanning electron microscopy images of different electroplating times at current densities;

[0042] Fig.11 The morphological evolution diagram of lithium deposition and delithiation on the Cu2S NS@Cu foil current collector;

[0043] Fig.12 0.5 mA·cm -2 XPS analysis of SEI at different depths of Cu2S NS@Cu foil obtained by deposition at a current density of 1 h;

[0044] Fig.13 For Cu2S NS@Cu foil, Cu2S@Cu foil, CuNS@Cu foil and Cu foil at 1mA·cm -2 &1mAh·cm -2 Half-cell performance diagram under parameters (ether-based electrolyte);

[0045] Fig.14 For Cu2S NS@Cu foil at 1mA·cm -2 &1mAh·cm -2 Half-cell performance diagram under parameters (carbonate electrolyte);

[0046] Fig.15 The long cycle performance of LFP||Cu2S NS@Cu foil full battery at 0.5C and 1C;

[0047] Fig.16 The long cycle performance of NCM 811||Cu2S NS@Cu foil full battery at 0.5C;

[0048] Fig.17 The scanning electron microscope image of the Cu2S@Cu foil prepared in control example 1;

[0049] Fig.18This is the scanning electron microscope image of the CuNS@Cu foil prepared in control example 2. DETAILED DESCRIPTION

[0050] The present invention provides a novel copper foil current collector with vertically distributed Cu2S nanosheets on the surface. In the present invention, the thickness of the Cu2S nanosheet is preferably 5 to 15 nm, more preferably 8 to 12 nm; the height is preferably 1 to 3 μm, more preferably 1.5 to 2.5 μm. In the present invention, the Cu2S nanosheet is preferably a crystal; the Cu2S nanosheet is preferably a polygonal nanosheet.

[0051] The vertical nanosheet arrays distributed on the surface of the copper foil can increase the specific surface area of ​​the copper foil to an appropriate level. The stable nanosheet array structure alleviates the unlimited volume expansion of lithium metal while reducing the local current density, thereby achieving uniform charge distribution on the electrode surface, inhibiting the growth of lithium dendrites, and achieving ultra-smooth deposition of metallic lithium, providing a guarantee for the long-term stable cycle of lithium metal batteries.

[0052] In the initial stage of lithium metal deposition, the Cu2S nanosheets are converted into copper nanosheets covered with an ultra-thin Li2S interface layer (denoted as Li2S-CuNS@Cu foil) through an in-situ lithiation replacement reaction. The Li2S interface layer can adhere to the surface of lithium metal during the lithium electroplating process, thereby greatly suppressing the side reaction between the electrolyte and lithium metal. -5 S cm -1 ) can promote the vertical growth of metallic lithium, which is beneficial to homogenizing the lithium ion flux distribution and realizing the ultra-dense deposition of metallic lithium.

[0053] The present invention provides a method for preparing the novel copper foil current collector of the above scheme, comprising the following steps: placing the copper foil as a working electrode in a sodium hydroxide solution, performing anodization under constant current conditions, and vertically growing CuO nanosheets on the surface of the copper foil to obtain CuO NS@Cu foil;

[0054] The CuONS@Cu foil is sulfurized to obtain the novel copper foil current collector.

[0055] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.

[0056] The invention uses copper foil as a working electrode and places it in a sodium hydroxide solution, performs anodization under a constant current condition, and vertically grows CuO nanosheets on the surface of the copper foil to obtain CuO NS@Cu foil.

[0057] In the present invention, the copper foil is preferably a commercial copper foil.

[0058] Before placing the copper foil as a working electrode in a sodium hydroxide solution, the present invention preferably further comprises high temperature annealing of the copper foil; the temperature of the high temperature annealing is preferably 900-1100°C, more preferably 950-1050°C; the time is preferably 1-3h, more preferably 1.5-2.5h; the atmosphere is preferably an Ar-H2 mixed atmosphere; the volume ratio of Ar and H2 in the Ar-H2 mixed atmosphere is preferably 1:1. In the present invention, the flow rate of the Ar-H2 mixed atmosphere is preferably 80-150sccm, more preferably 100-120sccm. The present invention utilizes high temperature annealing to remove impurities on the surface of the copper foil.

[0059] In the present invention, the concentration of the sodium hydroxide solution is preferably 0.8 to 1.2 mol / L, more preferably 1.0 mol / L. In the present invention, the current of the anodic oxidation is preferably 0.1 to 0.3 mA·cm -2 , more preferably 0.20 to 0.26 mA·cm -2 The time is preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours. In the present invention, the counter electrode and reference electrode of the anodic oxidation are preferably copper rods. In the anodic oxidation process of the present invention, CuO nanosheets grow vertically on the surface of the copper foil to obtain CuONS@Cu foil.

[0060] In the present invention, the CuO NS@Cu foil is preferably washed with deionized water for multiple times, and then the CuO NS@Cu foil is sulfurized after natural drying.

[0061] In the present invention, the temperature of the sulfurization is preferably 80 to 150°C, more preferably 100 to 120°C; the time is preferably 5 to 12 minutes, more preferably 7 to 10 minutes. In the present invention, the sulfurization atmosphere is preferably an Ar-H2S mixed atmosphere, and the volume ratio of Ar to H2S in the Ar-H2S mixed atmosphere is preferably 8 to 12:1, more preferably 10:1. In the sulfurization process of the present invention, the CuO nanosheets are sulfurized into Cu2S nanosheets to obtain a new copper foil current collector.

[0062] Figure 1 Schematic diagram of the preparation of the novel copper foil current collector of the present invention. Figure 1 As shown, the present invention first uses copper foil as a working electrode and places it in a sodium hydroxide solution, performs anodization under constant current conditions, and vertically grows CuO nanosheets on the surface of the copper foil to obtain CuO NS@Cu foil; then, the CuO NS@Cu foil is sulfurized to obtain the novel copper foil current collector, which is recorded as Cu2SNS@Cu foil.

[0063] The present invention provides the use of the novel copper foil current collector described in the above scheme or the novel copper foil current collector prepared by the preparation method described in the above scheme in a lithium metal battery.

[0064] The present invention has no special requirements for the application process, and any application process well known in the art may be used.

[0065] The novel copper foil current collector provided by the present invention, its preparation method and its application in lithium metal batteries are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0066] Example 1

[0067] 1. Pretreatment of copper foil

[0068] The commercial copper foil was cut into suitable sizes and placed in a high temperature furnace for high temperature annealing. The annealing temperature was 1050°C, the annealing atmosphere was 100 sccm of Ar-H2 mixed atmosphere (the volume ratio of Ar and H2 was 1:1), and the annealing time was 2 h.

[0069] 2. Preparation of CuONS@Cu foil

[0070] The treated copper foil was fixed with a platinum clip as the working electrode and immersed in 1 mol L -1 The counter electrode and reference electrode were copper rods in a NaOH aqueous solution. Anodic oxidation was performed using a constant current technique under a three-electrode system with a current density of 0.26 mA cm -2 , time: 2h, and CuO NS@Cu foil was obtained.

[0071] 3. Preparation of Cu2S NS@Cu foil

[0072] The CuO NS@Cu foil was washed with deionized water for many times, dried naturally and placed in a high-temperature furnace for sulfurization. The sulfurization parameters were: sulfurization atmosphere Ar-H2S mixed atmosphere (the volume ratio of Ar to H2S was 10:1), sulfurization temperature was 100℃, and sulfurization time was 7min to obtain Cu2S NS@Cu foil.

[0073] Application Example 1

[0074] Metal lithium deposition design process:

[0075] A half-cell consisting of Li foil, Celgard 2400 separator and Cu2S NS@Cu foil was used to study lithium deposition. Among them, Li foil was used as reference electrode and counter electrode, and Cu2S NS@Cu foil prepared in Example 1 was used as working electrode. 40 μL of a mixed solution of 1,3-dioxolane (DOL) and methylal (DME) dissolved with 1M lithium bistrifluoromethylsulfonyl imide (LiTFSI) and 2wt% LiNO3 was added as an electrolyte (the volume ratio of DOL and DME was 1:1), and the battery was assembled in a glove box. The glove box was filled with argon gas so that the content of water and oxygen was <0.1ppm, and then the metal lithium was deposited by constant current electroplating; deposition conditions: first, 0.05 mA·cm -2 The Li2S-CuNS@Cu foil was obtained by activating the Li2S-CuNS@Cu foil for five cycles in the voltage range of 0.01-1 V with a current density of 1 mA·cm -2 Lithium deposition was performed at different current densities for different times. Figure 2 As shown in the figure, a is the constant current discharge / charge curve of the Cu2S NS@Cu foil electrode between 0.01 and 1.0 V for 5 cycles, showing the formation process of lithium sulfide; b is the CV curve of the prepared Cu2S NS@Cu foil||Li battery (0.5 mV s -1 ). Among them, the platform in Figure a and the peak in the shaded box in Figure b are typical features of lithium sulfide formation.

[0076] Comparative Example 1

[0077] The pretreated commercial copper foil was directly used as the current collector to study lithium deposition, and the pretreatment steps were the same as those in Example 1. The specific lithium deposition process was consistent with the Cu2S NS@Cu foil in Application Example 1.

[0078] Control trial 1

[0079] The annealed copper foil was sealed in a tube furnace and then heated to 400 °C in a H2S / Ar atmosphere for 0.5 h. After the temperature dropped to room temperature, the Cu2S@Cu foil was obtained.

[0080] Control trial 2

[0081] The obtained CuONS@Cu foil was annealed at 450°C for 3 h in an Ar / H2 atmosphere (the volume ratio of Ar and H2 was 1:1) to obtain a CuNS@Cu foil.

[0082] Battery performance test process:

[0083] Half-cell:

[0084] Electrochemical studies were performed using CR2025 type button cells (MTI Corporation), which were assembled in an argon-filled glove box (H2O < 0.1 ppm, O2 < 0.1 ppm). The lithium plating / stripping process was studied using a half-cell consisting of Li foil, Celgard 2400 separator and Cu2SNS@Cu foil of Example 1 (Cu2S@Cu foil of Control Experiment 1, CuNS@Cu foil and Cu foil of Control Experiment 2). Constant current experiments were performed on a Neware multichannel battery cycler. The cell was first charged at 0.05 mA cm -2 The electrodes were cycled five times in the voltage range of 0.01 to 1 V to stabilize the SEI and remove contamination from the electrodes. Then, the coulombic efficiency tests at different current densities and capacities were studied, and then the lithium was stripped to 1 V. The electrolytes for all half-cells were: a mixed solution of 1,3-dioxolane (DOL) and methylal (DME) dissolved with 1M lithium bistrifluoromethylsulfonyl imide (LiTFSI) and 2wt% LiNO3 (the volume ratio of DOL and DME was 1:1); or a mixed solution of (ethylene carbonate) EC / (diethyl carbonate) DEC / (dimethyl carbonate) DMC dissolved with 1M (lithium hexafluorophosphate) LiPF6 (v / v / v = 1:1:1).

[0085] Full Battery:

[0086] LFP (LiFePO4) full battery

[0087] The LFP powder, conductive carbon black and PVDF (mass ratio: 8:1:1) were fully stirred and mixed in N-methyl-2-pyrrolidone, and then evenly coated on aluminum foil and vacuum dried at 85℃ for 12h to obtain the LFP positive electrode. The LFP positive electrode was then paired with a lithium negative electrode of designed capacity (0.75mAh·cm -2 The electrolyte used in the LFP full cell is a mixed solution of 1,3-dioxolane (DOL) and methylal (DME) dissolved with 1M lithium bistrifluoromethylsulfonyl imide (LiTFSI) and 2wt% LiNO3 (the volume ratio of DOL and DME is 1:1). The LFP-based full cell has a voltage range of 2.3 to 3.9V (relative to Li / Li + ) voltage range.

[0088] NCM 811 full battery

[0089] LFP powder, conductive carbon black and PVDF (mass ratio: 96:2:2) were fully stirred and mixed in N-methyl-2-pyrrolidone, and then evenly coated on aluminum foil and dried in vacuum at 85 °C for 12 h to obtain NCM 811 positive electrode. Then, the NCM811 positive electrode was paired with a lithium negative electrode of designed capacity (10 mAh cm deposited). -2 The electrolyte of the full battery based on NCM 811 is a mixed solution of (ethylene carbonate) EC / (diethyl carbonate) DEC / (dimethyl carbonate) DMC (v / v / v=1:1:1) in which 1M (lithium hexafluorophosphate) LiPF6 is dissolved. The full battery based on NCM 811 has a voltage range of 2.7 to 4.4 V (relative to Li / Li + ) voltage range.

[0090] Structure and performance characterization:

[0091] 1. XRD characterization was performed on the copper foil, CuO NS@Cu foil, Cu2S NS@Cu foil of Example 1 and Li2S-CuNS@Cu foil of Application Example 1. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that CuO and Cu2S NS were successfully synthesized with good crystallinity, and lithium sulfide was successfully converted and synthesized after in situ lithiation.

[0092] 2. The CuO NS@Cu foil of Example 1 was observed by scanning electron microscope. The results are as follows: Figure 4-1 As shown. Figure 4-1 It can be seen that the CuO nanosheets are distributed in a three-dimensional vertical array. Figure 4-1 Magnified observation, the results are as follows Figure 4-2 As shown in Figure 1, it is further confirmed that the CuO nanosheets are distributed in a three-dimensional vertical array. The CuO NS@Cu foil of Example 1 was observed by transmission electron microscopy, and the results are as follows: Figure 4-3 As shown by Figure 4-3 It can be seen that the CuO nanosheets appear as polygonal nanosheets. Figure 4-4 This is a high-resolution transmission electron microscopy image of the CuO NS@Cu foil of Example 1, showing that the CuO nanosheets have good crystallinity.

[0093] 3. The Cu2S NS@Cu foil of Example 1 was observed by scanning electron microscope. The results are as follows: Figure 5-1 As shown. Figure 5-1 It can be seen that after sulfurization, the Cu2S nanosheets perfectly inherit the microstructure of CuO. Figure 5-1 Magnified observation, the results are as follows Figure 5-2 As shown. Figure 5-2It can be seen that after sulfurization, the Cu2S nanosheets are distributed in a vertical array. The Cu2S NS@Cu foil of Example 1 was observed by transmission electron microscopy, and the results are as follows Figure 5-3 As shown by Figure 5-3 It can be seen that the Cu2S nanosheets appear as polygonal nanosheets. Figure 5-4 This is a high-resolution transmission electron microscopy image of Cu2S nanosheets, showing that the Cu2S nanosheets have good crystallinity.

[0094] 4. Scanning electron microscopy observation of the Li2S-CuNS@Cu foil in Example 1 is performed. The results are as follows Figure 6-1 As shown, the enlarged image is Figure 6-2 As shown. Figure 6-1 and Figure 6-2 It can be seen that the microscopic morphology after lithiation is still a vertical array, and the thickness of the nanosheets is slightly increased, which means the formation of a lithium sulfide interface layer. Figure 6-3 This is a low-temperature transmission electron microscopy image of Li2S-CuNS@Cu foil. Figure 6-3 It can be seen that SEI is divided into two layers: the outer layer is organic component and the inner layer is lithium sulfide layer. Figure 6-4 This is a high-resolution cryogenic transmission electron microscopy image of Li2S-CuNS@Cufoil. Figure 6-4 It can be seen that the crystallinity of the lithium sulfide interface layer is good.

[0095] 5. Fig.12 0.5 mA·cm -2 XPS analysis of SEI at different depths of Cu2S NS@Cu foil deposited at a current density of 10000 for 1 h. + During the sputtering process, lithium sulfide is located below the organic components and is the main component of SEI.

[0096] 6. Figure 7 For the Cu2S NS@Cu foil in Application Example 1 at 1mA·cm -2 Scanning electron microscope image of electroplating for 10h at a current density of . Figure 7 It can be seen that the Cu2S NS@Cu foil achieves ultra-smooth metallic lithium deposition.

[0097] 7. Figure 8 j and k are the Cu2S NS@Cu foil in application example 1 at 1mA·cm -2 Scanning electron microscope cross-sectional images of Cu2S NS@Cu foil electroplated at a current density of 1 mA·cm -2Scanning electron microscope cross-sectional and plan views of the Cu2S NS@Cu foil after electroplating for 10 h at a current density of . From the cross-sectional and planar SEM, it can be seen that the lithium metal coating on the surface of the Cu2S NS@Cu foil is smooth and dense, and its thickness is close to the theoretical lithium foil thickness.

[0098] 8. Fig. 9 This is a scanning electron microscope image of the copper foil after pretreatment in Comparative Example 1. It can be seen that the surface morphology of the copper foil is smooth and flat.

[0099] 9. Fig.10 For comparative example 1, the copper foil is at 1 mA·cm -2 Scanning electron microscope images of different electroplating times under current density. Among them, a is electroplating for 1h, b is electroplating for 3h, c is electroplating for 5h, and d is electroplating for 10h. Fig.10 It can be seen that the lithium metal is deposited unevenly directly on the surface of the copper foil, and mainly exists in the form of lithium dendrites.

[0100] 10. Fig.11 Figure 2 shows the morphological evolution of lithium deposition and delithiation on the Cu2S NS@Cu foil current collector. -2 The current density was 10000, and the deposition time was 1h, 3h, 5h and 10h (b-e); after 50 cycles, the lithium was removed for 1h, 3h and 5h until the lithium was completely removed (f-i). It can be seen that no lithium dendrites and dead lithium were observed during the entire electroplating and delithiation process, and the deposited lithium was very dense. In addition, it can be seen from the cyclic morphology that the process has good reversibility, indicating that the utilization rate of lithium metal is high.

[0101] 11. Fig.17 This is the scanning electron microscope image of the Cu2S@Cu foil prepared in Control Example 1. It can be seen that a thin layer of cuprous sulfide is generated on the surface of the copper foil after one-step sulfidation. Fig.18 This is a scanning electron microscope image of the CuNS@Cu foil prepared in Control Example 2, showing that the surface of the copper foil is a 3D porous structure after thermal reduction.

[0102] 12. Fig.13 For Cu2S NS@Cu foil, Cu2S@Cu foil, CuNS@Cu foil and Cu foil at 1mA·cm -2 &1mAh·cm -2 Half-cell performance diagram under parameters. Fig.13It can be seen that Cu2SNS@Cu foil achieved an ultra-high coulombic efficiency (99.1%) cycle of more than 1100 cycles (ether electrolyte: 1M LiTFSI in DOL / DME with 2wt% LiNO3). In addition, although the high surface area and high quality SEI alone can improve battery performance, the improvement capacity is limited and needs to be coordinated to achieve excellent battery performance.

[0103] 13. Fig.14 For Cu2S NS@Cu foil at 1mA·cm -2 &1mAh·cm -2 Half-cell performance diagram under parameters. Fig.14 It can be seen that the Cu2S NS@Cu foil achieved an ultra-high coulombic efficiency (98.8%) of more than 300 cycles (carbonate electrolyte: 1M LiPF6EC / DEC / DMC).

[0104] 14. Fig.15 The long cycle performance of LFP||Cu2S NS@Cu foil full battery at 0.5C and 1C; Fig.16 The long cycle performance of NCM811||Cu2S NS@Cu foil full battery at 0.5C. It can be seen that Cu2S NS@Cu foil exhibits excellent electrochemical performance both in half-cell and full-cell.

[0105] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A copper foil current collector, characterized in that: Cu2S nanosheets are distributed vertically on the surface; the thickness of the Cu2S nanosheets is 5 to 15 nm; the height is 1 to 3 μm; and the Cu2S nanosheets are crystals.

2. The method for preparing the copper foil current collector according to claim 1, characterized in that: The following steps are involved: A copper foil is placed as a working electrode in a sodium hydroxide solution and anodized under constant current conditions to vertically grow CuO nanosheets on the surface of the copper foil to obtain CuO NS@Cu foil; The CuO NS@Cu foil is sulfurized to obtain the copper foil current collector.

3. The preparation method according to claim 2, characterized in that: The concentration of the sodium hydroxide solution is 0.8-1.2 mol / L.

4. The preparation method according to claim 2, characterized in that: The current of the anodic oxidation is 0.1-0.3 mA·cm -2 , time is 1 to 3 hours.

5. The preparation method according to claim 2, characterized in that: The sulfurization atmosphere is an Ar-H2S mixed atmosphere, and the volume ratio of Ar to H2S in the Ar-H2S mixed atmosphere is 8 to 12:

1.

6. The preparation method according to claim 2 or 5, characterized in that: The vulcanization temperature is 80-150° C., and the vulcanization time is 5-12 minutes.

7. The preparation method according to claim 2, characterized in that: Before placing the copper foil as a working electrode in a sodium hydroxide solution, the copper foil is also subjected to high-temperature annealing; the temperature of the high-temperature annealing is 900-1100°C, the time is 1-3 hours, and the atmosphere is an Ar-H2 mixed atmosphere; the volume ratio of Ar and H2 in the Ar-H2 mixed atmosphere is 1:

1.

8. Use of the copper foil current collector according to claim 1 or the copper foil current collector prepared by the preparation method according to any one of claims 2 to 7 in lithium metal batteries.

Citation Information

Patent Citations

  • Metal lithium negative electrode and preparation method thereof

    CN110660969A

  • Cuprous sulfide material with surface hydrophobicity and preparation method for cuprous sulfide material

    CN110714197A

  • Lithium metal composite negative electrode with lithium-philic and lithium-phobic gradient structure, and preparation method thereof

    CN111599983A

  • Rambutan shell-like 3D lithium-philic composite current collector, lithium metal anode and preparation and application thereof

    CN111816881A

  • Modified copper current collector for negative electrode of lithium metal battery and preparation method of modified copper current collector

    CN114464814A