A method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube
Through multi-pass cold rolling, strict oil removal, heat treatment and straightening process steps, the UNS N10276 Hastelloy seamless heat exchange pipe has been solved, and the inspection pass rate, low material rate and surface quality of the UNS N10276 Hastelloy alloy seamless heat exchange pipe has been solved, achieving high precision, High-quality product manufacturing, suitable for mass production.
Patent Information
- Application Number
- CN202211547147.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-05
AI Technical Summary
In the prior art, the domestic manufacturing of UNS N10276 Hastelloy seamless heat exchange pipes has problems such as low pass rate, low material rate, low dimensional accuracy and poor internal and external surface quality.
A manufacturing method including multiple passes of cold rolling, strict oil removal, heat treatment, straightening, ultrasonic vortex current and pipe cutting is adopted. Through detailed process steps and parameter control, the high precision and high quality of the pipe are ensured. Specific steps include: initial inspection and grinding of hot extrusion blanks, three intermediate products cold rolling and oil removal, finished products cold rolling and oil removal, multiple heat treatments and straightening, ultrasonic vortex and pipe cutting, and finally surface inspection and finish.
The first-time inspection pass rate, material yield, dimensional accuracy and internal and external surface quality of UNS N10276 Hastelloy seamless heat exchange pipe has been improved, ensuring the stable mechanical properties of the product and suitable for mass production.
Smart Images

Figure BDA0003979827030000071 
Figure BDA0003979827030000081 
Figure BDA0003979827030000082
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a seamless pipe, in particular to a method for preparing a UNS N10276 Hastelloy seamless heat exchange pipe, and belongs to the technical field of material processing. Background Art
[0002] UNS N10276 alloy is a tungsten-containing nickel-chromium-molybdenum alloy with extremely low silicon-carbon content. It is an alloy with extremely excellent corrosion resistance, good resistance to chloride ion corrosion and strong acid corrosion, and is one of the few materials that can be used in concentrated sulfuric acid solutions. UNS N10276 alloy condenser equipment is widely used in corrosive environment equipment projects such as power plant desulfurization and denitrification, fine chemicals, and PTA, and UNS N10276 seamless heat exchange tubes are extremely important components of their equipment.
[0003] In the past, UNS N10276 alloy seamless heat exchange tubes were mainly imported from abroad, with long delivery cycles and high prices, so their domestic manufacturing is particularly important. At present, domestically produced N10276 alloy seamless heat exchange tubes have problems such as low first-time inspection pass rate, low material yield rate, low dimensional accuracy, and poor internal and external surface quality.
[0004] Patent CN103212603A provides a manufacturing process for Hastelloy stainless steel seamless pipes: (1) inspecting the material and performing the first pickling of the material, (2) grinding, rolling and drawing, and degreasing the pickled billet, (3) judging whether it meets the requirements of the finished product, if not, performing solid solution heat treatment, straightening, pickling of the intermediate product and repeating step 2, (4) if so, performing solid solution heat treatment, straightening, cutting, pickling, and inspection of the finished product. The patent mentions the grinding of the billet in step (2), but does not provide a detailed description of the methods for inspecting and grinding the billet and inspecting and grinding the intermediate product. The grinding quality is Important factors affecting the quality of the final product, especially the grinding quality of the tube billet and the grinding quality of the previous cold rolling of the finished product, cannot be improved through effective inspection methods, and the grinding efficiency cannot be improved while ensuring the grinding quality, and the qualified rate and yield rate of the finished tube cannot be improved. Step (2) of the patent mentions the combined production of rolling and drawing. Although the combined production of cold rolling and cold drawing can improve production efficiency, cold drawing will reduce the dimensional accuracy and inner wall quality of the product, and the need to remove the cold drawing head will also lead to a decrease in the final yield rate. The finished tube produced in this way has low dimensional accuracy, poor surface quality and low yield rate. Patent CN103212603A provides a manufacturing step for Hastelloy stainless steel seamless steel pipe, but lacks a manufacturing method for high-precision UNS N10276 Hastelloy heat exchange tube. Based on this, a production process for N10276 alloy seamless heat exchange tube that can overcome the above-mentioned difficulties is developed. It is a technical problem that technicians in this field need to solve urgently to develop N10276 seamless heat exchange tube with high one-time inspection pass rate, high yield rate, high dimensional accuracy, good internal and external surface quality, and physical and chemical properties that meet standard technical requirements. Summary of the invention
[0005] The technical problem to be solved by the present invention is to propose a manufacturing method of UNSN10276 Hastelloy seamless heat exchange tube in view of the shortcomings of the above prior art. The products produced by the method have a high one-time inspection pass rate, a high yield rate, high dimensional accuracy, good inner and outer surface quality, stable organizational performance, strong practicality, and are conducive to batch production.
[0006] The technical solution of the present invention to solve the above technical problems is:
[0007] A method for manufacturing a UNS N10276 Hastelloy seamless heat exchange tube specifically comprises the following steps:
[0008] (1) Conduct incoming material inspection and internal and external surface grinding of UNS N10276 hot extrusion billets, specifically: initial inspection + grinding + re-inspection of hot extrusion billets, and PT sampling during re-inspection;
[0009] (ii) subjecting the tube blank obtained in step (i) to three passes of intermediate product cold rolling, wherein after each pass of cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, inspected and ground, wherein:
[0010] When the intermediate product is cold rolled in three passes, the cold rolling deformation of each intermediate product is 45%-65%, the rolling speed is controlled at ≤60 times / min, the feed amount is ≤3mm / time, and the Q value is ≥1.10;
[0011] The three-pass intermediate product cold rolling is as follows:
[0012] In the first cold rolling, the outer diameter deviation after rolling is controlled within ±0.3mm, and the wall thickness deviation is controlled within ±0.3mm;
[0013] In the second cold rolling, the outer diameter deviation after rolling is controlled within ±0.2mm, and the wall thickness deviation is controlled within ±0.2mm;
[0014] In the third cold rolling, the outer diameter deviation after rolling is controlled within ±0.15mm, and the wall thickness deviation is controlled within ±0.15mm.
[0015] The specific process of degreasing the intermediate product is: degreasing in an alkali tank → rinsing → soaking in a hot water tank → degreasing in an acid tank → rinsing → inspection;
[0016] The intermediate products are heat treated in roller hearth furnaces with an oxidizing atmosphere.
[0017] The first heat treatment temperature is controlled at 1160±10℃, and the holding time is wall thickness×2min;
[0018] During the second heat treatment, the heat treatment temperature is controlled to be 1160±10℃, and the holding time is wall thickness×2.5min;
[0019] During the third heat treatment, the heat treatment temperature is controlled to be 1160±10℃, and the holding time is wall thickness×3min;
[0020] (iii) cold rolling the third pass steel tube obtained in step (ii);
[0021] When rolling finished products, the cold rolling deformation is 55%-70%, the rolling speed is controlled at ≤120 times / min, the feed amount is ≤2mm / time, and the Q value is ≥0.85;
[0022] When the finished product is cold rolled, the outer diameter deviation after rolling is controlled within ±0.05mm, and the wall thickness deviation is controlled within ±0.05mm;
[0023] (iv) degreasing the steel pipe obtained in step (iii);
[0024] The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection;
[0025] (5) subjecting the steel pipe obtained in step (4) to finished product heat treatment;
[0026] The finished product heat treatment is carried out in a bright furnace, and the atmosphere in the furnace is ammonia decomposition or pure hydrogen;
[0027] When the finished product is heat treated, the heat treatment temperature is controlled to be 1130±10℃, and the holding time is wall thickness×3min;
[0028] (6) straightening the steel pipe obtained in step (5);
[0029] (VII) subjecting the steel pipe obtained in step (VI) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests during pipe cutting;
[0030] When cutting the finished product pipe, it is preferred to use the old ACC type angle grinder and small grinding wheel in the prior art to cut the pipe, which has good effect, fast speed, and can meet the requirement of cutting margin +0-3mm;
[0031] (VIII) The steel pipe obtained in step (VII) is subjected to finished product surface inspection, cleaning, spray marking and finishing processes, and finally packaged and stored.
[0032] The technical solution further defined in the present invention is:
[0033] Furthermore, in the aforementioned method for manufacturing UNS N10276 Hastelloy alloy seamless heat exchange tube, in step (ii) of degreasing the intermediate product, the components of the solution in the alkali cylinder are controlled to be degreased in the alkali cylinder in a mass ratio of: degreasing agent: water = 1:7, alkali cylinder temperature: 70-80°C, alkali cylinder immersion time: 30-50min;
[0034] When degreasing the acid cylinder, the components of the solution in the acid cylinder are controlled to be calculated by mass ratio: HF: 1% + HNO3: 10-15%, the remainder is tap water, the sum of the above components is 100%, the acid cylinder temperature: 60°C, and the pickling time: 5min.
[0035] In the aforementioned method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube, during the straightening of the intermediate product in step (ii):
[0036] The first straightening control speed is ≤5m / min, the curvature after straightening is ≤1.5mm / m, and the outer diameter deviation after straightening is ±0.03mm;
[0037] The speed of the second and third straightening passes is controlled at ≤8m / min, the curvature after straightening is ≤1.0mm / m, and the outer diameter deviation after straightening is ±0.02mm.
[0038] In the aforementioned method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube, during the step (ii) of cutting the intermediate product and pickling:
[0039] The components of the solution in the acid cylinder are calculated by mass ratio: HF: 5-8%, HNO3: 10-15%, and the balance is tap water. The sum of the above components is 100%. The temperature of the acid cylinder is controlled at: 60℃;
[0040] The first and second pickling times are both controlled within 10 minutes, and the third pickling time is controlled within 15 minutes.
[0041] In the aforementioned method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube, during the step (ii) of intermediate product inspection and grinding:
[0042] The first and second pass steel pipes are inspected after pickling by visual inspection and endoscope inspection.
[0043] The third pass of steel pipe inspection after pickling is done by visual inspection after internal and external polishing + endoscope inspection one by one.
[0044] In the aforementioned method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube, when the finished tube is degreased in step (iv), the mass ratio of the solution in the alkali cylinder is, degreasing agent: water = 1:6.5, the alkali cylinder temperature is: 40-60°C, the alkali cylinder immersion time is: 30-60min, and the inner wall is wiped clean with a cloth strip for 3-5 times.
[0045] In the aforementioned method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube, in step (six), when straightening the finished tube, the straightening machine controls the speed to be ≤10m / min, the curvature after straightening is ≤0.5mm / m, and the outer diameter deviation after straightening is ±0.01mm.
[0046] In the aforementioned method for manufacturing the UNS N10276 Hastelloy alloy seamless heat exchange tube, in step (seven), the first ultrasonic qualified rate is ≥97%, and the first eddy current qualified rate is 100%.
[0047] In the aforementioned method for manufacturing UNS N10276 Hastelloy seamless heat exchange tube, the surface inspection in step (eight) includes visual inspection and dimensional inspection, and the qualified rate is ≥99%. The dimensional accuracy of the finished tube is controlled as follows: outer diameter ±0.05mm, wall thickness ±0.05mm, and the inner and outer surfaces of the finished tube are smooth, and the inner and outer wall roughness Ra≤0.5.
[0048] In the aforementioned method for manufacturing the UNS N10276 Hastelloy alloy seamless heat exchange tube, the finished tube obtained by room temperature tensile test has the following results: yield strength of 310-360 MPa, tensile strength of 740-770 MPa, and elongation after fracture ≥65%.
[0049] The beneficial effects of the present invention are:
[0050] The present invention adopts 4 cold rolling passes, 1-3 passes are intermediate cold rolling, the cold rolling deformation is controlled at 45%-65%, and 4 passes are finished cold rolling, the cold rolling deformation is controlled at 55%-70%, so that the grains are fully broken, and a finer grain size can be obtained after heat treatment. 1-3 passes of intermediate cold rolling ensure the surface quality by strictly controlling the feed amount ≤3mm / time, and by controlling the Q value ≥1.10, the deformation is more uniform, thereby improving the dimensional accuracy. Similarly, the finished cold rolling ensures the surface quality and dimensional accuracy by strictly controlling the feed amount ≤2mm / time and controlling the Q value ≥0.85.
[0051] The present invention provides a method for degreasing intermediate products in 1-3 passes, including strictly controlling the ratio of the alkali cylinder and the acid cylinder, the temperature and time to ensure the degreasing quality and avoid the risk of carburization during heat treatment. The present invention provides a method for degreasing finished products in 4 passes, which uses an alkali cylinder for degreasing, a clean water cylinder for soaking, acetone for wiping the outer surface and a cloth strip soaked in acetone to clean the inner wall. The alkali cylinder ratio, temperature and time and the inner and outer wall cleaning method are strictly controlled to ensure the degreasing quality of the finished pipe and ensure that the finished product bright heat treatment has no risk of carburization.
[0052] The 1-3 intermediate product solid solution heat treatment of the present invention is carried out in a roller hearth furnace, the atmosphere in the furnace is slightly oxidizing, the heat treatment temperature is 1160±10°C, the cold rolling work hardening is eliminated, the seamless pipe has good plasticity, and the subsequent cold rolling forming is convenient. The 4-pass finished product solid solution heat treatment is carried out in a bright furnace, the atmosphere in the furnace is ammonia decomposition or pure hydrogen, the heat treatment temperature is 1130±10°C, and while obtaining good organization and comprehensive mechanical properties, the surface color of the heat exchange tube is bright and the consistency of the overall color is guaranteed.
[0053] The invention specifies the straightening machine model, straightening speed, straightness and outer diameter deviation range after straightening, especially specifies the use of a plastic roller straightening machine for finished product straightening, specifies the straightening speed ≤ 10 m / min, ensures the curvature while avoiding the risk of iron rod straightening scratches and marks, and ensures the quality of finished product straightening. Strictly specifying the outer diameter deviation range after straightening, especially after finished product straightening, can effectively avoid the risk of outer diameter deviation caused by straightening, thereby improving dimensional accuracy.
[0054] The present invention stipulates the flattening amount and the middle cutting method. During the middle cutting, manual measurement is required to mark the middle position before cutting the pipe, and visual inspection is not allowed. This can reduce the risk of the intermediate and finished pipes being underlength, and improve the final finished product inspection pass rate and the final yield rate.
[0055] The present invention provides a method for pickling of 1-3 intermediate products, including strictly controlling the ratio of the acid cylinder, the temperature and the time to ensure the pickling quality. In this method, the inner and outer walls of the N10276 intermediate product pipe washed out have no oxide scale, and there is no tendency of over-acidification, so as to avoid the oxide scale not being washed clean, resulting in backwashing or polishing, which will extend the production cycle and reduce the production efficiency. Some small crack defects after polishing are not easy to be found visually, which will lead to poor grinding quality, and finally lead to crack extension, and the qualified rate of finished product ultrasonic and surface inspection will be reduced.
[0056] The present invention specifies methods for grinding and repairing hot extrusion billets and intermediate steel pipes. The PT re-inspection and random sampling of the hot extrusion billets is to avoid residual cracks. The hot extrusion billets and 1-3 passes of intermediate products are ground with endoscopes one by one in order to more accurately and efficiently treat inner wall defects. Ultrasound is performed during the 3 passes of intermediate product grinding in order to strictly control the quality of incoming materials before cold rolling of the finished products, thereby improving the final ultrasonic qualification rate, surface inspection qualification rate and final yield rate.
[0057] The method of the present invention solves the problems of low first-time inspection pass rate, low material yield rate, low dimensional accuracy and poor inner and outer surface quality by strictly limiting the process optimization of UNS N10276 seamless heat exchange tube. The products produced by the method have high first-time inspection pass rate, high material yield rate, high dimensional accuracy, good inner and outer surface quality, stable mechanical properties, strong practicality, and are conducive to batch production.
[0058] The N10276 seamless heat exchange tube prepared by the method of the present invention has a first ultrasonic qualified rate of ≥97%, a first eddy current qualified rate of 100%, a first table inspection (visual inspection + size inspection) qualified rate of ≥99%, and a comprehensive first inspection qualified rate (ultrasonic qualified rate×eddy current qualified rate×table inspection qualified rate) of ≥96%.
[0059] The yield rate of N10276 seamless heat exchange tubes prepared by the method of the present invention (hot extrusion billet→finished tube) is ≥89%.
[0060] The N10276 seamless heat exchange tube prepared by the method of the present invention can meet the following dimensional accuracy: outer diameter ±0.05mm, wall thickness ±0.05mm.
[0061] The N10276 seamless heat exchange tube prepared by the method of the present invention has smooth inner and outer surfaces, and the color is consistent, and the inner and outer wall roughness Ra≤0.5.
[0062] The room temperature tensile test of the N10276 seamless heat exchange tube prepared by the method of the present invention shows that the yield strength is 310-360 MPa, the tensile strength is ≥740 MPa, and the elongation after fracture is ≥65%. DETAILED DESCRIPTION
[0063] The following is a further detailed description of the method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube in conjunction with the examples, but the embodiments of the invention are not limited to the following examples.
[0064] Example 1
[0065] This embodiment provides a method for manufacturing a UNS N10276 Hastelloy seamless heat exchange tube, which specifically includes the following steps:
[0066] (I) Conduct an initial inspection of the UNS N10276 hot extrusion billets, and preliminarily characterize the defects of the billets and their grinding and repairing methods. For the hot extrusion defects on the outer surface of the billets, spot grinding and external polishing are performed. For the internal burrs and transverse cracks on some billets, internal polishing is performed. After the billets are ground, they are re-inspected. During the re-inspection, random inspections are performed for PT. Only qualified products can be circulated. Unqualified products are re-grinded;
[0067] (ii) subjecting the tube blank obtained in step (i) to three passes of intermediate product cold rolling, wherein after each pass of cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, inspected and ground;
[0068] (iii) cold rolling the third pass steel tube obtained in step (ii);
[0069] (iv) degreasing the steel pipe obtained in step (iii);
[0070] The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection;
[0071] (5) subjecting the steel pipe obtained in step (4) to finished product heat treatment;
[0072] (6) straightening the steel pipe obtained in step (5);
[0073] (VII) subjecting the steel pipe obtained in step (VI) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests during pipe cutting;
[0074] (VIII) The steel pipe obtained in step (VII) is subjected to finished product surface inspection (including visual and dimensional inspection), cleaning, spray marking and finishing processes, and finally packaged and stored.
[0075] In this embodiment 1, the cold rolling process of UNS N10276 seamless heat exchange tubes strictly controls the cold rolling deformation of intermediate products and finished products, selects a reasonable rolling speed and a relatively small feed amount to ensure the quality of the inner and outer surfaces, and controls the Q value to ensure the uniformity of the structure in the wall thickness direction, thereby improving the dimensional accuracy and improving the quality of the inner wall. The specific cold rolling parameters are shown in Table 1 below, and the technical requirements for dimensional accuracy and actual dimensions are shown in Table 2. It can be seen from Table 2 that the dimensional accuracy of the intermediate product tubes and finished tubes at each pass meets the internal control requirements of our company, and the dimensional accuracy of the finished tubes is much higher than the ASME SB622-2019 standard requirements.
[0076] Table 1 UNS N10276 cold rolling parameters
[0077]
[0078] Table 2 UNS N10276 technical requirements dimensional accuracy and actual measured dimensions
[0079]
[0080] In this embodiment 1, the specific process of degreasing the intermediate product of UNS N10276 seamless heat exchange tube is: degreasing by alkali cylinder → flushing → soaking in hot water cylinder → degreasing in acid cylinder → flushing → inspection, and the main control requirements of degreasing the intermediate product are shown in Table 3; the degreasing steps of the finished tube are: degreasing by soaking in alkali cylinder → soaking in clean water cylinder → wiping the outer surface → taping the inner wall with cloth strips → inspection, and the main control requirements of degreasing the finished tube are shown in Table 4. The inner and outer surfaces of the tube degreasing by the above method are clean and free of oil stains, and there is no risk of carburization during heat treatment.
[0081] Table 3 Main control requirements for UNS N10276 intermediate product degreasing process
[0082]
[0083] Table 4 Main control requirements for degreasing process of UNS N10276 finished pipe
[0084]
[0085] In this embodiment 1, the heat treatment of the intermediate products of UNS N10276 seamless heat exchange tubes is carried out in a roller hearth furnace with an oxidizing atmosphere; the heat treatment of the finished products is carried out in a bright furnace with an atmosphere of ammonia decomposition or pure hydrogen. The heat treatment system is as shown in Table 5.
[0086] Table 5 UNS N10276 heat treatment system
[0087]
[0088] It can be seen from Table 5 that the 1st to 3rd pass solution heat treatment is carried out in a roller hearth furnace, the atmosphere in the furnace is slightly oxidizing, the furnace has 6 temperature zones, the first three temperature zones T01-T03 are heating zones, the last three temperature zones T04-T06 are insulation zones, the heat treatment temperature is 1160℃, the insulation time is 19min, 15min and 10min respectively, and the cooling method is water cooling. The finished product heat treatment is bright heat treatment, the atmosphere in the furnace is ammonia decomposition, the furnace has 5 temperature zones, T01-T02 is the heating zone, T03-T05 is the insulation zone, the heat treatment temperature is 1130℃, the insulation time is 6min, and the cooling method is water jacket cooling.
[0089] In this embodiment 1, the straightening parameters of the intermediate and finished products of UNS N10276 seamless heat exchange tubes are shown in Table 6. By specifying the straightening machine model, straightening speed, straightness and outer diameter deviation range after straightening, especially the straightening of finished products, it is specified that a plastic roller straightening machine is used, and the straightening speed is specified to be ≤10m / min. While ensuring the curvature, the risk of iron rod straightening causing scratches and marks can be avoided, thereby ensuring the quality of finished product straightening. Strictly specifying the outer diameter deviation range after straightening, especially after straightening of finished products, can effectively avoid the risk of outer diameter deviation caused by straightening, thereby improving dimensional accuracy.
[0090] Table 6 UNS N10276 straightening parameters
[0091]
[0092]
[0093] In this embodiment 1, the requirements for cutting the intermediate products and finished products of UNS N10276 seamless heat exchange tubes are shown in Table 7. By strictly controlling the amount of flattening and strictly following the middle cutting method, the middle position must be manually measured and marked before cutting the tube, and visual inspection is not allowed. This can reduce the risk of the intermediate products and finished products being under-lengthened, and improve the final product inspection pass rate and the final yield rate.
[0094] Table 7 UNS N10276 pipe cutting requirements
[0095] Specification equipment Pipe cutting requirements Intermediate product cutting φ108×9.5 Grinding machine Flat head requirements: Strictly control the amount of flat heads, no overcutting allowed Intermediate product cutting φ76×6 Grinding machine Middle cutting requirements: measure the length and mark the middle position, visual inspection is not allowed Intermediate product cutting φ48×3.3 Grinding machine Middle cutting requirements: measure the length and mark the middle position, visual inspection is not allowed Finished pipe cutting φ25.4×2 ABC type angle grinder Cutting requirements: remove blind areas, cut to size, cut margin +0~3mm
[0096] In this embodiment 1, the main control requirements for pickling of the intermediate product of UNS N10276 seamless heat exchange tube are shown in Table 8 below, including strict control of the ratio of the acid tank, temperature and time to ensure the pickling quality. In this method, the inner and outer walls of the N10276 intermediate product tube washed out have no oxide scale, and there is no tendency of over-acidification, which avoids the oxide scale not being washed clean, resulting in backwashing or polishing, which will extend the production cycle and reduce production efficiency. Some small crack defects after polishing are not easy to be found visually, which will lead to poor grinding quality, and ultimately lead to crack extension, and the qualified rate of finished product ultrasonic and surface inspection will decrease.
[0097] Table 8 Main control requirements for pickling process of UNS N10276 intermediate products
[0098]
[0099] In this embodiment 1, the inspection and grinding and repairing operation requirements of the hot extrusion billet and intermediate product tubes of UNS N10276 seamless heat exchange tubes are shown in Table 9 below. The purpose of re-inspection and random sampling of the hot extrusion billet is to ensure that there are no residual cracks. The purpose of grinding and repairing the hot extrusion billet and the 1-3 passes of intermediate products with an endoscope is to more accurately and efficiently treat the inner wall defects. The purpose of performing ultrasound during the 3 passes of intermediate product grinding and repair is to strictly control the quality of the incoming materials before the finished product is cold rolled, thereby improving the final ultrasonic qualified rate, surface inspection qualified rate and final yield rate.
[0100] Table 9 UNS N10276 grinding and repairing operation requirements
[0101]
[0102] In this Example 1, the ultrasonic, eddy current, water pressure, visual and dimensional inspection results of the finished UNS N10276 seamless heat exchange tube are shown in Table 10. It can be seen from Table 10 that the ultrasonic pass rate of the N10276 seamless heat exchange tube produced by the production method is as high as 97.37%, the eddy current and water pressure pass rates are both 100.00%, the dimensional inspection pass rate is also 100.00%, the dimensional accuracy is much higher than the dimensional accuracy specified in the ASME SB622-2019 standard, the visual inspection pass rate is as high as 99.41%, and the one-time inspection pass rate is as high as 96.80%.
[0103] Table 10: Ultrasonic, eddy current, water pressure, visual and dimensional inspection of finished UNS N10276 pipes
[0104]
[0105] In this embodiment 1, the yield rate of UNS N10276 seamless heat exchange tubes is shown in Table 11. 400 hot extrusion billets are put into the batch, 8 finished products are made from 1 batch, weighing 33310 kg, and 3016 finished products weighing 29810 kg, with a yield rate of up to 89.49%.
[0106] Table 11 UNS N10276 yield rate
[0107]
[0108] The test method for room temperature tensile properties of finished pipes is ASTM E8, and the test results are shown in Table 12. From Table 12, it can be seen that the mechanical properties of the N10276 pipes manufactured by this method are excellent, the yield strength of 13 furnace batches is 310-360Mpa, which is higher than the ASMESB622-2019 standard requirement of ≥283Mpa, the tensile strength is stable at 740-770Mpa, which is higher than the standard requirement of ≥690Mpa, and the elongation after fracture is ≥65%, which is much higher than the standard requirement of ≥40%.
[0109] Table 12 UNS N10276 finished tube room temperature tensile properties
[0110]
[0111] The present invention solves the problems of low first-time inspection pass rate, low material yield rate, low dimensional accuracy and poor inner and outer surface quality by strictly limiting the process optimization of UNS N10276 seamless heat exchange tube. It can be seen from Tables 10-13 that the products produced by the method have a high first-time inspection pass rate, a high material yield rate, high dimensional accuracy, good inner and outer surface quality, stable mechanical properties, strong practicality, and are conducive to batch production.
[0112] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A method for manufacturing a UNS N10276 Hastelloy seamless heat exchange tube, characterized in that: The specific steps include: (I) Conduct incoming material inspection and internal and external surface grinding of UNS N10276 hot extrusion billets, specifically: initial inspection + grinding + re-inspection of hot extrusion billets, and PT sampling during re-inspection; (ii) subjecting the tube blank obtained in step (i) to three passes of intermediate product cold rolling, wherein after each pass of cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, inspected and ground, wherein: When the intermediate product is cold rolled in three passes, the cold rolling deformation of each intermediate product is 45%-65%, the rolling speed is controlled at ≤60 times / min, the feed amount is ≤3mm / time, and the Q value is ≥1.10; The three-pass intermediate product cold rolling is as follows: In the first cold rolling, the outer diameter deviation after rolling is controlled within ±0.3mm, and the wall thickness deviation is controlled within ±0.3mm; In the second cold rolling, the outer diameter deviation after rolling is controlled within ±0.2mm, and the wall thickness deviation is controlled within ±0.2mm; In the third cold rolling, the outer diameter deviation after rolling is controlled within ±0.15mm, and the wall thickness deviation is controlled within ±0.15mm; The specific process of degreasing the intermediate product is: degreasing in an alkali tank → rinsing → soaking in a hot water tank → degreasing in an acid tank → rinsing → inspection; When degreasing the alkali cylinder, the components of the solution in the alkali cylinder are controlled to be calculated by mass ratio: degreasing agent: water = 1:7, alkali cylinder temperature: 70-80℃, alkali cylinder soaking time: 30-50min; When degreasing the acid cylinder, the components of the solution in the acid cylinder are controlled by mass ratio: HF: 1% + HNO3: 10-15%, the balance is tap water, the sum of the above components is 100%, the acid cylinder temperature: 60℃, the pickling time: 5min; When straightening the intermediate product: The first straightening speed is controlled at ≤5m / min, the curvature after straightening is ≤1.5mm / m, and the outer diameter deviation after straightening is ±0.03mm; the second and third straightening speeds are controlled at ≤8m / min, the curvature after straightening is ≤1.0mm / m, and the outer diameter deviation after straightening is ±0.02mm; When cutting and pickling the intermediate product: The components of the solution in the acid tank are calculated by mass ratio: HF: 5-8%, HNO3: 10-15%, and the balance is tap water. The sum of the above components is 100%. The temperature of the acid tank is controlled at: 60℃; The first and second pickling times are controlled within 10 minutes, and the third pickling time is controlled within 15 minutes; The intermediate products are heat treated in a roller hearth furnace with an oxidizing atmosphere. The first heat treatment temperature is controlled at 1160±10℃, and the holding time is wall thickness×2min; During the second heat treatment, the heat treatment temperature is controlled to be 1160±10℃, and the holding time is wall thickness×2.5min; During the third heat treatment, the heat treatment temperature is controlled to be 1160±10℃, and the holding time is wall thickness×3min; (iii) cold rolling the third pass steel tube obtained in step (ii) into finished product; When rolling finished products, the cold rolling deformation is 55%-70%, the rolling speed is controlled at ≤120 times / min, the feed amount is ≤2mm / time, and the Q value is ≥0.85; When the finished product is cold rolled, the outer diameter deviation after rolling is controlled within ±0.05mm, and the wall thickness deviation is controlled within ±0.05mm; (iv) degreasing the steel pipe obtained in step (iii); The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection; The mass ratio of the solution in the alkali tank is degreasing agent: water = 1:6.5, the temperature of the alkali tank is 40-60℃, the soaking time of the alkali tank is 30-60min, and the inner wall is wiped clean with a cloth strip for 3-5 times; (V) subjecting the steel pipe obtained in step (IV) to finished product heat treatment; The finished product heat treatment is carried out in a bright furnace, and the atmosphere in the furnace is ammonia decomposition or pure hydrogen; When the finished product is heat treated, the heat treatment temperature is controlled to be 1130±10℃, and the holding time is wall thickness×3min; (vi) straightening the steel pipe obtained in step (v); When straightening finished pipes, use a plastic roller straightener to control the speed to ≤10m / min, the curvature after straightening to ≤0.5mm / m, and the outer diameter deviation after straightening to ±0.01mm; (VII) subjecting the steel pipe obtained in step (VI) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests when cutting the pipe; (VIII) The steel pipes obtained in step (VII) are subjected to surface inspection, cleaning, spray marking and finishing processes, and finally packaged and stored.
2. The method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube according to claim 1, characterized in that: During the inspection and grinding of intermediate products in step (ii): The first and second pass steel pipes are inspected after pickling by visual inspection and endoscope inspection. The third pass of steel pipe inspection after pickling is carried out by visual inspection after internal and external polishing + endoscope inspection one by one.
3. The method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube according to claim 1, characterized in that: In the step (VII), the first ultrasonic qualified rate is ≥97%, and the first eddy current qualified rate is 100%.
4. The method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube according to claim 1, characterized in that: The surface inspection in step (eight) includes visual inspection and dimensional inspection, with a qualified rate of ≥99%. The dimensional accuracy of the finished tube is controlled as follows: outer diameter ±0.05mm, wall thickness ±0.05mm, the inner and outer surfaces of the finished tube are smooth, and the inner and outer wall roughness Ra≤0.
5.
5. The method for manufacturing the UNS N10276 Hastelloy seamless heat exchange tube according to claim 1, characterized in that: The room temperature tensile test of the manufactured finished pipe shows the following results: yield strength 310-360 MPa, tensile strength 740-770 MPa, and elongation after fracture ≥ 65%.