Method, material and application of biocarbonized magnesium oxide solidification geological materials based on urea prehydrolysis

Urea prehydrolysis technology improves the utilization rate of active magnesium oxide and urea, solves the problem of insufficient material strength in the existing technology, realizes the production of efficient biocarbonized magnesium oxide materials, and provides a feasible solution for cement replacement.

CN115925379BActive Publication Date: 2024-10-01NANJING UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310003073.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-10-01
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

The utilization rate of active magnesium oxide and urea in the existing microbial-induced activated magnesium oxide carbonization technology is low, resulting in insufficient material strength and inability to effectively replace traditional cement.

Method used

By mixing urea with urease-producing bacteria liquid for pre-hydrolysis, carbonate and ammonium radicals are generated, mixed with active magnesium oxide and geological materials to form a fluid slurry, and left to stand and cured under specific conditions to improve urea and activity Magnesium oxide utilization and material strength.

Benefits of technology

Significantly improves the strength of biocarbonized magnesium oxide materials, the strength increase can exceed 400%, delays the setting time, reduces the pH value, broadens the applicability of the material, and provides technical support for the replacement of cement and concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115925379B_ABST
    Figure CN115925379B_ABST
Patent Text Reader

Abstract

The present invention discloses a method, material and application of biocarbonized magnesium oxide solidified geological materials based on urea prehydrolysis. The method comprises the following steps: mixing urea and bacterial solution for prehydrolysis, wherein the concentration of the urea is 1-4 mol / L, the bacterial solution contains urease-producing bacteria and has been cultivated to a stable period, and the prehydrolysis time is 2-24 hours; mixing geological materials and active magnesium oxide into a solid mixture, wherein the mass of the active magnesium oxide is 5-15% of the mass of the geological materials; mixing the prehydrolyzed mixed solution and the solid mixture to form a slurry with fluidity; wherein the mass ratio of the prehydrolyzed mixed solution to the solid mixture is 65:35-78:22. The method of the present invention increases the utilization rate of urea and active magnesium oxide, improves the performance of biocarbonized active magnesium oxide, reduces the pH value and fluidity of the sample, delays the coagulation of the sample, and improves the strength of the sample.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method, material and application of biocarbonized magnesium oxide solidified geological materials based on urea prehydrolysis. Background Art

[0002] Cement has made a significant contribution to urban construction since its birth, but cement production not only consumes a lot of energy, but is also accompanied by problems such as high pollution and high emissions. At present, my country is working hard to achieve the ambitious goals of carbon peak in 2030 and carbon neutrality in 2060. Continuing to use a large amount of high-carbon emission cement is inconsistent with this goal. It is necessary to continue to seek an efficient and clean emerging solidification method.

[0003] As an emerging solidification technology, microbial induced carbonization of activated magnesium oxide mainly utilizes urease-producing microorganisms to hydrolyze urea and produce carbonate and ammonium ions, and generates basic magnesium carbonate (HMCs) with magnesium hydroxide produced by hydration of activated magnesium oxide. This mineral has extremely strong cementitious properties. It can not only cement itself, but also cement various aggregates to form materials with good mechanical properties. Compared with cement, the firing temperature of activated magnesium oxide cement is low (750℃ vs 1400℃). Microbial induced carbonization of activated magnesium oxide will be conducive to achieving the goal of carbon neutrality. This technology has been studied to a certain extent in the repair of concrete cracks and tailings treatment. However, the current utilization rate of materials such as activated magnesium oxide and urea is low, resulting in low strength, which causes a lot of material waste. Summary of the invention

[0004] In view of the above technical problems, the purpose of the present invention is to provide a method, material and application of biocarbonized magnesium oxide solidification geological materials based on urea prehydrolysis.

[0005] The first aspect of the present invention provides a method for solidifying geological materials by biocarbonized magnesium oxide based on urea prehydrolysis, comprising the following steps:

[0006] Mixing urea and bacterial solution for pre-hydrolysis, wherein the concentration of the urea is 1-4 mol / L, the bacterial solution contains urease-producing bacteria and has been cultivated to a stable period, and the pre-hydrolysis time is 2-24 hours;

[0007] Mixing geological materials and active magnesium oxide into a solid mixture, wherein the mass of the active magnesium oxide is 5 to 15% of the mass of the geological materials;

[0008] The pre-hydrolyzed mixed liquid and the solid mixture are mixed to form a fluid slurry; wherein the mass ratio of the pre-hydrolyzed mixed liquid to the solid mixture is 65:35 to 78:22.

[0009] Preferably, the solid mixture further contains a hydrating agent, and the mass of the hydrating agent is 1-6% of the total mass of the solid mixture. More preferably, the mass of the hydrating agent is 1-5%, further 2-5%, and further 2-3% of the total mass of the solid mixture. The hydrating agent further promotes the hydration of magnesium oxide and the release of magnesium ions.

[0010] More preferably, the hydrating agent includes one or both of magnesium acetate tetrahydrate and sodium hexametaphosphate.

[0011] Preferably, the pre-hydrolysis time is 6 to 12 hours. The strength of the material reaches a peak value within the range of 6 to 12 hours, and the increase in strength can exceed 400%.

[0012] Preferably, the pre-hydrolysis is carried out at 25-35°C.

[0013] Preferably, the concentration of urea is 2-4 mol / L; more preferably 2-3 mol / L.

[0014] Preferably, the urease-producing bacteria is one or both of Bacillus pasteurianus and Sporosarcina pasteurianus.

[0015] The geological material includes but is not limited to construction waste, silt, sand, loess and other soils, and some other granular materials, and the pH of the geological material should not exceed 9.5. In a specific embodiment, the geological material is construction waste aggregate pre-treated into granular form, and the construction waste aggregate is mainly waste bricks for construction. The construction waste aggregate is pre-treated into granular form, and the particle size is ≤5mm, preferably ≤2mm.

[0016] Preferably, the method further comprises the steps of: injecting the slurry into a mold, a mine goaf, a foundation or a roadbed, and curing the slurry at 25-35°C and a relative humidity of 90-95%. More preferably, the slurry is injected into the roadbed, foundation or slope to be treated, and curing the slurry after leveling the slurry.

[0017] In a specific and preferred embodiment, the method is implemented as follows:

[0018] Mixing urea and bacterial solution cultivated to a stable period and pre-hydrolyzing them at 25-35° C. for 6-12 hours; the concentration of the urea is 2-4 mol / L; the bacterial solution includes one or two of Bacillus pasteurianus and Sporosarcina pasteurianus, and the bacterial concentration OD600 value is greater than 1.25, and the urease activity is greater than 7U;

[0019] Mix construction waste aggregate, active magnesium oxide and a hydrating agent to form a solid mixture; the particle size of the construction waste aggregate is ≤5mm; the purity of the active magnesium oxide is greater than 90%, the mesh size is less than 300 meshes, the citric acid indicator activity is 20-25s, the hydration ratio is greater than 80%, and the mass of the active magnesium oxide is 7.5-12.5% ​​of the mass of the construction waste aggregate; the hydrating agent includes one or two of magnesium acetate tetrahydrate and sodium hexametaphosphate, and the mass of the hydrating agent is 1-6% of the total mass of the solid mixture;

[0020] The pre-hydrolyzed mixed liquid and the solid mixture are mixed in a mass ratio of 68:32 to 72:28 to form a slurry with fluidity;

[0021] The slurry is injected into a mold, a mine goaf, a foundation or a roadbed, and is kept stationary for curing at 25 to 35° C. and a relative humidity of 90 to 95%.

[0022] The second aspect of the present invention provides a material made by the method for solidifying geological materials by biocarbonization of magnesium oxide based on urea prehydrolysis.

[0023] Preferably, the material comprises a cement substitute, a concrete substitute, a foundation or roadbed material or a mine goaf filling material.

[0024] The third aspect of the present invention provides an application of the material in the preparation of cement substitutes, concrete substitutes, foundation or roadbed materials, and mine goaf filling.

[0025] The present invention adopts the above solution, which has the following advantages compared with the prior art:

[0026] In the method of the present invention, 1-4 mol / L of urea is used, and the urea is mixed with a urease-producing bacterial solution that has been cultivated to a stable period and pre-hydrolyzed for 2-24 hours, so that the urea is hydrolyzed in advance, the carbonization of the active magnesium oxide is promoted, the utilization rate of urea and the active magnesium oxide is improved, and the performance of the biocarbonized active magnesium oxide is improved, the pH value and fluidity of the sample are reduced, the coagulation of the sample is delayed, and the strength of the sample is improved (the increase in strength can exceed 400%). The method has the characteristic of early strength, which broadens the applicability of the biocarbonized active magnesium oxide technology and provides favorable technical support for it as an alternative material for cement and concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solution of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0028] Figure 1 The particle size distribution curves of construction waste particles and activated magnesium oxide are shown.

[0029] Figure 2 The curves showing the unconfined compressive strength of the samples of Comparative Example 1 and Examples 1 to 4 changing with the curing time are shown.

[0030] Figure 3 The curves showing the change of urea utilization rate with curing time in Comparative Example 1 and Examples 1 to 4 are shown.

[0031] Figure 4 Fourier infrared images of the samples of Comparative Example 1 and Examples 1 to 4 are shown.

[0032] Figure 5a and Figure 5b The scanning electron microscope images of the samples of Example 2 and Comparative Example 1 are shown respectively.

[0033] Figure 6 The curves showing the unconfined compressive strength of the samples of Comparative Example 2 and Examples 5 and 6 as a function of curing time are shown.

[0034] Figure 7 The curves showing the change of urea utilization rate with curing time in Comparative Example 2 and Examples 5 and 6 are shown. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention.

[0036] The method provided in this embodiment can significantly improve the utilization of active magnesium oxide and urea in the biocarbonized active magnesium oxide technology. It is an efficient and clean cement replacement bonding method that ensures high utilization rates of active magnesium oxide and urea. Based on this technology, construction waste, sludge, shield waste residue and other construction waste are used as aggregates for mine filling, roadbed and pavement construction, urban furniture, slopes, tunnel drainage and other ancillary infrastructure construction. This technology can adjust the fluidity, setting time, strength, etc. of the slurry prepared with construction waste according to engineering needs.

[0037] This embodiment provides a method for significantly improving the utilization rate of active magnesium oxide and urea, which comprises the following steps:

[0038] A. Mix urea and a high urease activity bacterial solution cultivated to a stable stage at 30 degrees Celsius, and then allow the solution to stand for curing, so that the microorganisms can hydrolyze the urea and generate a large amount of carbonate and ammonium.

[0039] Preferred high-urease-producing microorganisms include, but are not limited to, Bacillus pasteurianus and Sporosarcina pasteurianus. The concentration of the selected microorganism is OD 600 The value should be greater than 1.25, and the urease activity should be greater than 7U (1U=mmol urea / (L·min)). The microbial culture medium can use a sterile culture medium, including but not limited to yeast extract, ammonium sulfate and Tris-base buffer. After the culture medium is sterilized, it is inoculated with Bacillus pasteurianus at an inoculum amount of 1-10%, and cultured with shaking for 24 hours to form the bacterial liquid.

[0040] As the pre-hydrolysis time increases, the concentration of carbonate ions increases first rapidly, then slowly, then gradually stabilizes, and then decreases relatively. It is worth noting that the hydrolysis of urea mainly occurs within 24 hours after mixing.

[0041] The urea concentration should be in the range of 1-4 mol / L, preferably in the range of 2-4 mol / L. The prehydrolysis time should be set in the range of 2-24 hours, preferably in the range of 6-12 hours.

[0042] B. Mix aggregates such as construction waste with active magnesium oxide in a certain proportion, and add a certain amount of hydrating agent to form a solid mixture.

[0043] The mass ratio of the solid mixture to the liquid mixture should be in the range of 65:35-78:22, preferably in the range of 68:32-72:28.

[0044] The proportion of magnesium oxide should be 5-15% of the mass ratio of the cured aggregate, preferably within the range of 10±2.5%. Excessive magnesium oxide will cause the volume expansion of the generated crystals, reduce the strength of the sample, lead to the proportion of active magnesium oxide participating in the reaction, and increase the cost. Too little active magnesium oxide will reduce the curing effect.

[0045] The purity of active magnesium oxide should be more than 90%, the mesh size should be less than 300 mesh, its citric acid activity should be 20-25s, and the hydration ratio should be more than 80%.

[0046] The hydrating agent includes, but is not limited to, magnesium acetate tetrahydrate and other weakly acidic hydrating agents, which promote the dissolution of magnesium hydroxide, the release of magnesium ions and the hydration of magnesium oxide.

[0047] The grading of aggregates such as construction waste should be good, and the maximum particle size should not exceed 5mm.

[0048] The specimen should be maintained at a temperature between 25 and 35°C and a relative humidity between 90 and 95%.

[0049] C. The mixed solution pre-hydrolyzed in step A and the solid mixture in step B are then stirred and mixed to prepare a fluid slurry.

[0050] D. Then, according to the needs of engineering practice, it is injected into mining goaf, roadbed, urban furniture molds and other engineering practice areas such as slope tunnels that need to be solidified, and then it flows by itself or hardens in various restricted areas. Its strength gradually increases, and finally forms a hardened body with strength and bearing engineering loads.

[0051] This method improves the utilization rate of the mixed urea and activated magnesium oxide, and also improves the performance of biocarbonized activated magnesium oxide. Specifically, the pre-hydrolysis technology reduces the pH value and fluidity of the sample, delays the coagulation of the sample, and improves the strength of the sample. This broadens the applicability of biocarbonized activated magnesium oxide technology and provides favorable technical support for its use as an alternative material for cement and concrete.

[0052] Compared with the biochar magnesium oxide gel without prehydrolysis treatment, the prehydrolysis gel has the following properties: its pH can decrease to a certain extent but the decrease is small, about 0.1, and the pH value does not show an obvious change trend with the increase of prehydrolysis time. Its setting time has increased to a certain extent with the extension of prehydrolysis time, and the initial setting time of the non-prehydrolysis sample is only 1 hour. After 6 to 12 hours of prehydrolysis treatment, the initial setting time exceeds 10 hours and the final setting time exceeds 15 hours. Within the range of 2 to 24 hours of prehydrolysis time, its setting time first increases and then decreases but is still higher than that of the non-prehydrolysis sample. The fluidity (consistency and slump) decreases monotonically with the increase of prehydrolysis time. The strength of the material increases first and then decreases with the prehydrolysis time, reaching a peak value in the range of 6-12 hours. The increase in strength can exceed 400%. In addition, the method provided in this article has the characteristics of early strength, and the 28-day curing strength in each prehydrolysis time increases less than the 3-day curing strength. The carbonate ions in the mixed solution can promote the carbonization of brucite or redissolved magnesium ions, and more basic magnesium carbonate is formed compared to the sample without pre-hydrolysis, wherein the basic magnesium carbonate is mainly in the form of D / H two minerals. The improvement of the sample performance can be attributed to the fact that the carbonate and ammonium ions in the mixed solution can be significantly increased after pre-hydrolysis, and the hydrolysis of urea in the mixed solution and the utilization of urea in the subsequent biological carbonization magnesium oxide reaction are improved. The ammonium ions in the mixed solution can promote the hydration of active magnesium oxide and the dissolution of magnesium hydroxide formed therefrom.

[0053] This embodiment significantly improves the utilization rate of active magnesium oxide and urea in the sample that participate in the reaction by adjusting the prehydrolysis time, under the premise of minimally increasing the material cost. In addition, adjusting the prehydrolysis time can change the performance of the sample before and after solidification, greatly improving its mechanical properties, and can meet the needs of various types of engineering construction. It can also adjust various types of energy according to engineering practice, providing a feasible adjustment measure for different needs.

[0054] The raw materials used in the following examples and comparative examples are as follows:

[0055] The curing aggregate is construction waste (≤2mm, with good particle size distribution);

[0056] The magnesium oxide content of activated magnesium oxide is 99%, the citric acid activity is 25s, and the hydration ratio is 75%.

[0057] The particle size distribution curves of construction waste particles and activated magnesium oxide are shown in Figure 1 .

[0058] Example 1

[0059] (1) Urea was mixed with a bacterial solution (OD600 = 1.3, urease activity = 10 U) cultured to the stable phase and pre-hydrolyzed for 2 hours at a temperature of 30° C. The initial concentration of urea in the mixed solution was 4 M.

[0060] (2) The dried construction waste is mixed evenly with the active magnesium oxide, wherein the mass of the active magnesium oxide accounts for 10% of the total mass of the construction waste and the magnesium oxide.

[0061] (3) The bacterial liquid-urea mixed solution that has reached the pre-hydrolysis time is stirred and mixed with the uniformly mixed construction waste-activated magnesium oxide mixture, and the mass ratio of solid to liquid is 70:30 to form a fluid paste slurry. The pH value, setting time, and slump of the paste are tested and the measured data are shown in Table 1.

[0062] (4) Then fill it into the place to be cured or the sample preparation mold and carry out a certain period of curing (30 degrees Celsius, relative humidity 95%). The curing time is 3 days, 7 days, 14 days, and 28 days. The sample is tested for unconfined compressive strength. The sample after the mechanical property test is crushed, and the carbonate content in the sample is tested by the acid washing method, and the urea utilization rate in the mixture is calculated based on it. The test results are shown in Figure 2 To Figure 5.

[0063] Example 2

[0064] The difference between this embodiment and embodiment 1 is that the pre-hydrolysis time is 6 hours; the rest is the same as embodiment 1.

[0065] Example 3

[0066] The difference between this embodiment and embodiment 1 is that the pre-hydrolysis time is 12 hours; the rest is the same as embodiment 1.

[0067] Example 4

[0068] The difference between this embodiment and embodiment 1 is that the pre-hydrolysis time is 24 hours; the other aspects are the same as embodiment 1.

[0069] Comparative Example 1

[0070] The difference between Comparative Example 1 and Example 1 is that the pre-hydrolysis time is 0 hours, and the rest is the same as Example 1. That is, after urea is mixed with the bacterial solution cultivated to the stable period and the prepared solid mixture is added, no pre-hydrolysis treatment is performed.

[0071] The slurry properties of the samples of Comparative Example 1 and Examples 1 to 4 are shown in Table 1.

[0072] Table 1

[0073]

[0074] As shown in Table 1, compared with the biochar magnesium oxide gel without pre-hydrolysis treatment in Comparative Example 1, the pre-hydrolysis treated gels of Examples 1 to 4 have the following properties: the pH can decrease to a certain extent but the decrease is small, about 0.1, and the pH value does not show an obvious change trend with the increase of pre-hydrolysis time. The initial setting time of the non-pre-hydrolyzed sample of Comparative Example 1 is only about 1 hour; after 6-12 hours of pre-hydrolysis treatment, the initial setting time exceeds 10 hours, and the final setting time exceeds 15 hours; within the range of 2-24 pre-hydrolysis time, its setting time increases first and then decreases, but it is still higher than the non-pre-hydrolyzed sample of Comparative Example 1. The fluidity (slump) decreases monotonically with the increase of pre-hydrolysis time.

[0075] Figure 2 The curves showing the unconfined compressive strength of the samples of Comparative Example 1 and Examples 1 to 4 as a function of curing time are shown. Figure 2 It can be seen that the strength of the material increases first and then decreases with the pre-hydrolysis time, reaching a peak value in the range of 6-12 hours. The increase in strength can exceed 400%. In addition, the method of the embodiment has the characteristic of early strength, and the 28-day curing strength in each pre-hydrolysis time increases less than the 3-day curing strength.

[0076] Figure 3 The curves showing the change of urea utilization rate with curing time in Comparative Example 1 and Examples 1 to 4 are shown. Figure 3 It can be seen that the urea utilization rates of Examples 1 to 4 gradually increase and are all greater than that of Comparative Example 1.

[0077] Figure 4 The Fourier infrared images of the samples of Comparative Example 1 and Examples 1 to 4 are shown. Figure 5a and Figure 5b The scanning electron microscope images of the samples of Example 2 and Comparative Example 1 are shown respectively. The carbonate ions in the mixed solution can promote the carbonization of brucite or redissolved magnesium ions, and more basic magnesium carbonate is formed compared with the sample without pre-hydrolysis, wherein the basic magnesium carbonate is mainly in the form of D / H minerals.

[0078] Example 5

[0079] The difference between this embodiment and embodiment 1 is that: (1) the pre-hydrolysis time is 6 hours; 1 wt% of magnesium acetate tetrahydrate and 1 wt% of sodium hexametaphosphate are also added to the solid mixture; the rest is the same as embodiment 1.

[0080] Example 6

[0081] The difference between this embodiment and embodiment 1 is that: (1) the pre-hydrolysis time is 24 hours; 1 wt% of magnesium acetate tetrahydrate and 1 wt% of sodium hexametaphosphate are also added to the solid mixture; the rest is the same as embodiment 1.

[0082] Comparative Example 2

[0083] The difference between Comparative Example 2 and Example 1 is that: (1) the pre-hydrolysis time is 0 hours; 1 wt% of magnesium acetate tetrahydrate and 1 wt% of sodium hexametaphosphate are also added to the solid mixture; the rest is the same as Example 1.

[0084] The slurry properties of the samples of Comparative Example 2 and Examples 5 and 6 are shown in Table 2.

[0085] Table 2

[0086]

[0087] Figure 6 The curves showing the unconfined compressive strength of the samples of Comparative Example 2 and Examples 5 and 6 as a function of curing time are shown.

[0088] Figure 7 The curves showing the change of urea utilization rate with curing time in Comparative Example 2 and Examples 5 and 6 are shown.

[0089] Refer to Table 2 and Figure 6 to Figure 7The coupling of magnesium acetate tetrahydrate and sodium hexametaphosphate has the effect of promoting the hydration of active magnesium oxide and releasing magnesium ions. This phenomenon reduces the pH value of the sample, delays the coagulation of the sample, and promotes the flow of the sample. In addition, the magnesium ions in the sample can promote the biocarbonization reaction of active magnesium oxide, increase the utilization rate of urea, increase the amount of basic magnesium carbonate generated, and improve the mechanical properties of the sample.

[0090] In addition, compared with the performance of the pre-hydrolyzed samples of Examples 1 to 4, the addition of admixtures in Examples 5 and 6 can reduce the pH value of the samples, increase fluidity, and delay the coagulation and hardening of the samples.

[0091] The above embodiment is only for illustrating the technical concept and features of the present invention, and is a preferred embodiment. Its purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and it cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for solidifying geological materials by biocarbonized magnesium oxide based on urea prehydrolysis, characterized in that: The steps include: Mixing urea and bacterial solution for pre-hydrolysis, wherein the concentration of the urea is 1-4 mol / L, the bacterial solution contains urease-producing bacteria and has been cultivated to a stable period, and the pre-hydrolysis time is 2-24 hours; Mixing geological materials and activated magnesium oxide into a solid mixture, wherein the mass of the activated magnesium oxide is 5-15% of the mass of the geological materials; the solid mixture also contains a hydrating agent, the mass of the hydrating agent is 1-6% of the total mass of the solid mixture, and the hydrating agent includes one or two of magnesium acetate tetrahydrate and sodium hexametaphosphate; The pre-hydrolyzed mixed liquid and the solid mixture are mixed to form a fluid slurry; wherein the mass ratio of the pre-hydrolyzed mixed liquid to the solid mixture is 65:35 to 78:

22.

2. The method according to claim 1, characterized in that The pre-hydrolysis time is 6 to 12 hours; the pre-hydrolysis is carried out at 25 to 35°C.

3. The method according to claim 1, characterized in that The concentration of the urea is 2-4 mol / L; the urease-producing bacteria are one or both of Bacillus pasteurianus and Sporosarcina pasteurianus.

4. The method according to claim 1, characterized in that The geological material is selected from one or more combinations of construction waste, sludge, and soil, and the pH of the geological material does not exceed 9.

5.

5. The method according to claim 1, characterized in that The method further comprises the following steps: injecting the slurry into a mold, a mine goaf, a foundation or a roadbed, and curing the slurry at 25-35° C. and a relative humidity of 90-95%.

6. The method according to claim 1, characterized in that The method is specifically implemented as follows: The urea and the bacterial solution cultivated to the stable period are mixed and pre-hydrolyzed at 25-35°C for 6-12 hours; the concentration of the urea is 2-4 mol / L; the bacterial solution includes one or two of Bacillus pasteurianus and Sporosarcina pasteurianus, and the bacterial concentration OD 600 The value is greater than 1.25, and the urease activity is greater than 7U; Mix construction waste aggregate, active magnesium oxide and a hydrating agent to form a solid mixture; the particle size of the construction waste aggregate is ≤5mm; the purity of the active magnesium oxide is greater than 90%, the mesh size is less than 300 meshes, the citric acid indicator activity is 20-25s, the hydration ratio is greater than 80%, and the mass of the active magnesium oxide is 7.5-12.5% ​​of the mass of the construction waste aggregate; the hydrating agent includes one or two of magnesium acetate tetrahydrate and sodium hexametaphosphate, and the mass of the hydrating agent is 1-6% of the total mass of the solid mixture; The pre-hydrolyzed mixed liquid and the solid mixture are mixed in a mass ratio of 68:32 to 72:28 to form a fluid slurry; The slurry is injected into a mold, a mine goaf, a foundation or a roadbed, and is kept stationary for curing at 25 to 35° C. and a relative humidity of 90 to 95%.

7. A material made by the method for solidifying geological materials based on biocarbonized magnesium oxide by urea prehydrolysis as claimed in any one of claims 1 to 6.

8. Use of the material as claimed in claim 7 in the preparation of cement substitutes, concrete substitutes, foundation or roadbed materials, and filling of mine goafs.

Citation Information

Cited By

  • Roadbed filling construction method for internal and external source carbonization reinforcement

    CN120844418A

  • Construction method for reinforcing collapsible loess foundation based on grouting carbonization-vibration densification cooperation

    CN122013759A