Preparation method and application of acidic soil conditioner based on electrolytic manganese slag and / or phosphogypsum

Acid soil improvement agents were prepared through the ball mill-calcination process of electrolytic manganese slag and phosphogypsum, which solved the problems of high energy consumption and soil plating in acidic soil improvement, achieved effective soil acidification relief and silicon nutritional replenishment, significantly improved soil pH value and exchangeable calcium and magnesium content.

CN115926796BActive Publication Date: 2024-11-26SOUTH CENTRAL UNIVERSITY FOR NATIONALITIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211544924.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-04
Publication Date
2024-11-26
Estimated Expiration
2042-12-04

AI Technical Summary

Technical Problem

The prior art has high energy consumption, soil slab and re-acidification when improving acidic soil, and frequent application of commonly used conditioning agents such as quicklime will lead to element imbalance.

Method used

Using electrolytic manganese slag and/or phosphogypsum as the basis, combined with the ball mill-calcination process, using alkali triggers and biochar to activate silicon in solid waste, to prepare an acidic soil modification agent, and obtain an improvement agent through low-temperature calcination and crushing, providing Silicon nutrients and increase soil pH.

Benefits of technology

Effectively alleviate soil acidification, reduce soil exchange acidity, improve the exchangeable calcium and magnesium content in the soil, significantly increase the soil pH value, and the process is simple, the energy consumption is low, and the use of alkali triggers is reduced, avoiding soil crunching and re-acidification .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003979361660000041
    Figure BDA0003979361660000041
  • Figure BDA0003979361660000042
    Figure BDA0003979361660000042
  • Figure BDA0003979361660000054
    Figure BDA0003979361660000054
Patent Text Reader

Abstract

The present invention relates to the technical field of acidic heavy metal contaminated soil remediation, and specifically to a preparation method and application of an acidic soil conditioner based on electrolytic manganese slag and / or phosphogypsum. With industrial solid wastes such as electrolytic manganese slag and phosphogypsum as the matrix, wollastonite powder is added to increase the silicon content, and the alkali excitation of sodium carbonate and the reducing property of biochar are used to activate the silicon in the industrial solid waste. The reducing property of biochar is used to make the industrial solid waste produce alkaline substances under high-temperature calcination, and the alkaline substances activate the silicon therein at high temperature, thereby achieving the effect of replacing part of the alkaline activator. Compared with the existing silicon fertilizer preparation process, the amount of alkaline activator used is relatively small, and the pH of the acidic soil conditioner prepared is greater than 10, which effectively reduces the exchangeable acidity of the soil and significantly increases the exchangeable calcium and magnesium content in the soil. Therefore, the soil conditioner can not only adjust the pH value of the soil, but also provide the soil with the required effective silicon nutrient element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of acidic heavy metal contaminated soil remediation, and in particular to a preparation method and application of an acidic soil conditioner based on electrolytic manganese slag and / or phosphogypsum. Background Art

[0002] Soil acidification will affect the physical and chemical properties of the soil, making the soil sticky and compacted, with poor ventilation, leading to a decline in soil quality. It will also affect the enzyme activity and photosynthetic performance of crops. In particular, the activity of heavy metals will also increase in strongly acidic soils. For example, heavy metal elements such as chromium and cadmium will be more easily released and absorbed by plants, further affecting the growth of crops.

[0003] Soil acidification refers to the phenomenon that the soil absorbs a certain amount of exchangeable hydrogen ions or aluminum ions due to the leaching of basic cations in the soil, turning it into aluminous soil. The strong leaching caused by heavy rainfall in the south (especially acid rain) leads to a large loss of basic ions such as potassium, calcium, and magnesium in the soil, and the H ions directly input by rainwater + and Al in rainwater and soil 3+ The H released by the reaction + Occupies the adsorption sites on the surface of soil colloids, thus exacerbating soil acidification. The large-scale application of nitrogen fertilizers, especially ammonium nitrogen fertilizers, on the surface of farmland soil causes a large amount of ammonium nitrogen to accumulate on the soil surface. Ammonium nitrogen is easily converted into nitrate nitrogen under aeration and oxidation conditions. During this conversion process, a large amount of hydrogen ions will be released, thereby destroying soil colloids, weakening the soil buffering capacity, accelerating the leaching of base ions, and accelerating soil acidification.

[0004] For a long time, applying acidic soil conditioners has been the easiest way to improve soil acidification. Common acidic soil conditioners include quicklime, limestone powder, etc. However, long-term application of quicklime can easily lead to soil compaction, imbalance of elements in the soil, and possible re-acidification of the soil. Therefore, when applying quicklime to improve soil acidification, it should not be applied frequently, and due to the large amount of application, a large amount of natural limestone needs to be mined and calcined, which will cause additional energy consumption and environmental problems.

[0005] At present, other conditioning agents have been disclosed to solve the above problems. For example, Chinese patent CN104496726B discloses a method for preparing soil conditioning agents by calcining phosphate tailings, phosphogypsum and potassium feldspar with coal at 900-1150°C for more than 1 hour, but the preparation process consumes a lot of energy. Chinese patent CN103436266B discloses a method for producing medium-amount acidic soil conditioning agents by using industrial calcium silicate board waste. Calcium silicate board, white mud, dolomite and auxiliary additives are calcined at 800-1100°C for 0.5-4 hours, and the energy consumption in the production process is still relatively large.

[0006] Chinese patent CN 106365899B discloses a method for preparing silicon fertilizer from industrial waste slag, wherein electrolytic manganese slag, fly ash, sodium carbonate and sodium hydroxide are ball-milled in proportion and then calcined and crushed by microwave at 750-850°C. The effective silicon content of the fertilizer reaches 21.05% after calcination at 800°C for 30 minutes. The ratio of the added alkali activator to the slag to be activated is about 0.38-0.5:1 during the production process. The amount of the alkali activator used is large, and the total production cost is high. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is first to provide a method for preparing an acidic soil conditioner based on electrolytic manganese slag and / or phosphogypsum. The prepared soil conditioner can not only effectively alleviate soil acidification, but also provide effective silicon nutrients for the soil.

[0008] A method for preparing an acidic soil conditioner based on electrolytic manganese slag and / or phosphogypsum, comprising the following steps:

[0009] (1) placing solid waste powder, alkaline activator, wollastonite powder and biochar in a planetary ball mill and fully milling them to obtain a silicon activated precursor;

[0010] (2) placing the silicon activated precursor obtained in step (1) in a muffle furnace for calcining for 0.5-1 h, with the calcination temperature controlled at 600-900° C. (preferably heating to 600-900° C. at a heating rate of 15° C. / min and then calcining for 0.5-1 h), cooling and then crushing to obtain an acidic soil conditioner;

[0011] Furthermore, the calcination temperature is 800° C. and the calcination time is 0.5 h.

[0012] The solid waste residue is phosphogypsum and / or electrolytic manganese slag.

[0013] Furthermore, the mass ratio of the solid waste powder, biochar, wollastonite powder and alkaline activator is (1-10):(0-5):(0-5):1, preferably (3-8):(0-1):(0-1):1;

[0014] Furthermore, the solid waste residue is a mixture of phosphogypsum and electrolytic manganese slag in a mass ratio of 3:1, and the mass ratio of the solid waste residue powder, biochar, wollastonite powder and alkaline activator is 8:1:0:1;

[0015] Furthermore, the solid waste is phosphogypsum, and the mass ratio of the solid waste powder, biochar, wollastonite powder and alkali activator is 3:1:0:1;

[0016] Furthermore, the ball milling conditions in step (1) are: ball-to-material ratio of 10:1, rotation speed of 300 r / min, and ball milling time of 0.5-1 h.

[0017] Furthermore, the alkaline activator is selected from at least one of calcium hydroxide, sodium hydroxide, sodium sulfate, calcium sulfate, sodium carbonate and water glass, preferably sodium carbonate.

[0018] In the above-mentioned process of preparing the acidic soil conditioner, the activation rate of silicon is 36.38%-79.4%, and the silicon activation rate = the ratio of the amount of soluble silicon in the final acidic soil conditioner to the total amount of silicon contained in the raw materials;

[0019] The present invention also provides application of the acidic soil conditioner obtained by the preparation method in acidic soil improvement.

[0020] Furthermore, the specific steps of the application are: mixing the acidic soil conditioner into the acidic soil according to the mass ratio of the acidic soil conditioner to the acidic soil = 0.1% to 5% (ie "application amount"), and the preferred application amount is 1.5%.

[0021] The present invention uses solid wastes such as electrolytic manganese slag and phosphogypsum as a matrix, adds wollastonite powder to increase the silicon content, and utilizes the alkali excitation of sodium carbonate and the reducing property of biochar to activate the silicon in the solid waste.

[0022] Compared with the prior art, the technical solution of the present application has the following advantages and beneficial effects:

[0023] (1) Compared with the prior art, the present invention adopts ball milling-calcination coupling technology, the production process is simple, and the calcination only needs to be performed at a temperature below 1000° C., and the calcination time is relatively short;

[0024] (2) Compared with the existing waste residue fertilizer processing technology, the effective utilization of silicon resources in phosphogypsum and manganese slag is achieved, the activation rate of silicon element is effectively improved, and the nutrient type contained is more, in addition to silicon, calcium, magnesium, phosphorus, potassium and other nutrients, it also contains nutrient sulfur;

[0025] (3) The present invention replaces part of the alkali activator with biochar, and utilizes the reducing property of biochar to produce alkaline substances under high-temperature calcination of waste residue. At the same time, the alkaline substances activate silicon in the waste residue at high temperature, thereby achieving the effect of replacing part of the alkali activator. Compared with the existing silicon fertilizer preparation process, the amount of alkali activator used is smaller, and the pH of the obtained acidic soil conditioner is greater than 10.

[0026] (4) The improver of the present invention has a good improvement effect on acidified soil. As the amount of improver applied increases, the soil pH value rises accordingly. An application amount of 1.5% can significantly increase the soil pH value. Secondly, it can effectively reduce the exchangeable acidity of the soil and significantly increase the exchangeable calcium and magnesium content in the soil. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is described in detail below in conjunction with specific embodiments.

[0028] The silicon content, silicon activation rate, etc. described in the present invention are all calculated in terms of SiO2, wherein silicon activation rate = amount of soluble silicon in the acidic soil conditioner / total amount of silicon contained in the raw materials*100%, wherein the total amount of silicon is the total silicon content calculated proportionally based on the chemical composition of each raw material, the amount of soluble silicon in the acidic soil conditioner = mass of the acidic soil conditioner × soluble silicon content, and the determination of soluble silicon content adopts the determination method of soluble silicon in calcium magnesium phosphate fertilizer in GB / T 20412-2021.

[0029] In the following examples, the electrolytic manganese slag EMR used refers to a solid waste residue produced during the electrolysis of manganese metal and does not contain anode electrolysis sludge, and its main components are shown in Table 1:

[0030] Table 1 Main chemical components of electrolytic manganese slag

[0031]

[0032] The phosphogypsum PG used is a by-product in the process of preparing phosphoric acid with wet sulfuric acid. Its main components are shown in Table 2:

[0033] Table 2 Main chemical components of phosphogypsum

[0034]

[0035] The main components of the wollastonite powder used are shown in Table 3 below, which is sieved through a 100-mesh sieve for later use:

[0036] Table 3 Main chemical components of wollastonite powder

[0037] Wollastonite powder CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> <![CDATA[SO3]]> <![CDATA[P2O5]]> <![CDATA[Fe2O3]]> Loss on ignition content(%) 47.555 36.768 3.158 0.10 0.092 0.033 0.19 12.024

[0038] The biochar used was pine cone biochar obtained from Huanggang, Hubei Province, which was washed, air-dried, and crushed, and then pyrolyzed at 500°C in a muffle furnace for 2 h. After cooling to room temperature, it was ground and passed through a 100-mesh sieve. The main components are shown in Table 4:

[0039] Table 4 Main chemical components of biochar

[0040] Biochar <![CDATA[CO2]]> <![CDATA[K2O]]> CaO MgO <![CDATA[SO3]]> <![CDATA[P2O5]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> content(%) 78.039 8.682 5.858 2.259 1.405 1.101 0.588 0.192

[0041] Example 1 A method for preparing an acidic soil conditioner based on phosphogypsum, the specific steps are as follows:

[0042] (1) drying the phosphogypsum raw material at 60° C. and then crushing the raw material through a 100-mesh sieve to obtain phosphogypsum powder;

[0043] (2) placing the dried phosphogypsum powder obtained in step (1) with wollastonite powder and sodium carbonate in a planetary ball mill at a mass ratio of 3:1:1, with a ball-to-material ratio of 10:1 and a rotation speed of 300 r / min, and ball milling for 0.5 h to obtain a silicon activated precursor;

[0044] (3) The silicon activated precursor obtained in step (2) is placed in a crucible and calcined in a muffle furnace. The temperature is raised from room temperature to 800° C. at a heating rate of 15° C. / min, and then calcined at this temperature for 30 min. After crushing, an acidic soil conditioner is obtained, the pH of which is 11.10 and the silicon activation rate is 36.38%.

[0045] The calculation method of silicon activation rate w in this embodiment is: In this embodiment, the amounts of phosphogypsum powder, wollastonite powder and sodium carbonate are 3g, 1g and 1g respectively, and the mass of the obtained acidic soil conditioner is 4.13g; the soluble silicon content of the acidic soil conditioner is detected to be 5.713%, and the amount of soluble silicon in the acidic soil conditioner is calculated as 4.13g×5.713%; The final calculated silicon activation rate is 36.38%. The following examples all calculate their respective silicon activation rates in the above manner;

[0046] The obtained acidic soil conditioner is applied to the acidified soil to be improved at a weight ratio of 0, 0.1%, 0.5% and 1.5% (i.e., 100 g of the acidified soil to be improved, 0, 0.1 g, 0.5 g and 1.5 g of the acidic soil conditioner respectively, and the application amount of other embodiments is the same as the above method), and then cultured at room temperature, and the exchangeable acidity (measured by the exchangeable aluminum content in the present invention), exchangeable magnesium content and exchangeable calcium content in the soil are measured on the 7th day and the 28th day respectively. The soil is stirred irregularly during the culture process, and water is added in time every 2 to 3 days to maintain the moisture in the soil at 60% of the maximum field water holding capacity. The pH value is determined according to the determination of soil pH value (NY / T1377-2007), the exchangeable acidity is determined according to the method in the following literature: Ji Tianwei, Shen Yue, Chen Sili, et al. "Research on the determination of soil exchangeable aluminum by plasma emission spectrometry" [J]. Journal of Zhejiang Agricultural Sciences, 2017, 29(8): 1347-1352, and the exchangeable calcium and magnesium are determined according to the method in the following literature: Zhao Yuting, Yu Peng, Zhu Hepeng, Jia Chengnan, Zhao Yunxia, ​​Deng Wanli. "Research on the determination method of exchangeable calcium and magnesium in different types of farmland soils" [J]. Agriculture and Technology, 2021, 041(006), 56-60. The above detection methods are adopted in the following examples and will not be repeated.

[0047] The relevant data results are recorded in Table 5 below, where the control group is the experimental group when the amount of the modifier applied is 0, that is, the original acidified soil to be improved (taken from Yuanbao Township, Lichuan City, Enshi, Hubei Province):

[0048] Table 5 Test results of Example 1 before and after improvement by acidic soil conditioner

[0049]

[0050]

[0051] As can be seen from Table 5, the modifier prepared by the present invention has a good improvement effect on acidified soil. As the amount of modifier applied increases, the soil pH value increases accordingly. An application amount of 1.5% can increase the soil pH value from 5.27 to 6.26; secondly, it can effectively reduce the exchangeable acidity of the soil and significantly increase the exchangeable calcium and magnesium contents in the soil. It was found through experiments that the exchangeable calcium and magnesium contents were basically stable after 28 days of cultivation.

[0052] Example 2 A method for preparing an acidic soil conditioner based on phosphogypsum, the specific steps are as follows:

[0053] (1) drying the phosphogypsum raw material at 60° C. and then crushing the raw material through a 100-mesh sieve to obtain phosphogypsum powder;

[0054] (2) placing the dried phosphogypsum powder, biochar and sodium carbonate obtained in step (1) in a planetary ball mill at a mass ratio of 3:1:1, with a ball-to-material ratio of 10:1 and a rotation speed of 300 r / min, and ball milling for 0.5 h to obtain a silicon activated precursor;

[0055] (3) The silicon activated precursor obtained in step (2) is placed in a crucible and calcined in a muffle furnace from room temperature to 800° C. at a heating rate of 15° C. / min, and calcined at this temperature for 30 min. After crushing, an acidic soil conditioner is obtained, the pH of which is 11.05 and the silicon activation rate is 79.40%.

[0056] (4) In order to verify the role of biochar, a control group was set up. In other words, except for not adding biochar, the other conditions were the same as steps (1) to (3) of Example 2. The pH of the obtained acidic soil conditioner was 11.48, and the silicon activation rate was 46.27%, which was significantly lower than 79.40% when biochar was added in step (3) of Example 2.

[0057] (5) Based on steps (1) to (3) of Example 2, the mass ratios of phosphogypsum powder, biochar and sodium carbonate were changed to 3:2:0, 3:0:2, 3:0.5:1 and 3:1:0, respectively. The silicon activation rates of the prepared acidic soil conditioners were 33.50%, 73.38%, 49.12% and 22.82%, respectively, which were also significantly lower than 79.40% in step (3) of Example 2. This shows that increasing the content of biochar can effectively increase its silicon activation rate, and when the content of the alkali activator is further increased, its silicon activation rate can also be greatly improved.

[0058] This may be due to the reducing property of biochar, which causes the waste slag to produce alkaline substances under high-temperature calcination. The alkaline substances can activate the silicon in the waste slag at high temperatures and act as an alkali activator, thereby achieving the purpose of replacing part of the alkali activator with biochar.

[0059] The acidic soil conditioner prepared in step (3) of Example 2 was applied to the acidified soil to be improved at a weight ratio of 0, 0.1%, 0.5%, and 1.5%, and then after cultivation at room temperature, the exchangeable acidity, exchangeable magnesium content, and exchangeable calcium content were measured on the 7th and 28th days, respectively. The soil was stirred irregularly during the cultivation process, and water was replenished every 2 to 3 days to maintain the moisture in the soil at 60% of the maximum field water holding capacity. The relevant data results are recorded in Table 6 below, where the control group is the experimental group when the amount of the conditioner applied is 0, that is, the original acidified soil to be improved (taken from Yuanbao Township, Lichuan City, Enshi, Hubei Province):

[0060] Table 6 Test results of Example 2 before and after improvement by acidic soil conditioner

[0061]

[0062] As can be seen from Table 6, the acidic soil conditioner prepared by the present invention has a good improvement effect on acidified soil. As the amount of the conditioner applied increases, the soil pH value rises accordingly. An application amount of 1.5% can increase the soil pH value from 5.27 to 6.62; secondly, it can effectively reduce the exchangeable acidity of the soil and significantly increase the exchangeable calcium and magnesium content in the soil. It was found through experiments that the exchangeable calcium and magnesium content is basically stable after 28 days of cultivation. Example 3 A method for preparing an acidic soil conditioner based on electrolytic manganese slag, the specific steps are as follows:

[0063] (1) drying the electrolytic manganese slag raw material at 60° C. and then crushing it through a 100-mesh sieve to obtain electrolytic manganese slag powder;

[0064] (2) placing the dried electrolytic manganese slag powder, wollastonite powder and sodium carbonate obtained in step (1) in a planetary ball mill at a mass ratio of 3:1:1, with a ball-to-material ratio of 10:1 and a set speed of 300 r / min, and ball milling for 0.5 h to obtain a silicon activated precursor;

[0065] (3) The silicon activated precursor obtained in step (2) is placed in a crucible and calcined in a muffle furnace from room temperature to 800° C. at a heating rate of 15° C. / min, and calcined at this temperature for 30 min. After crushing, an acidic soil conditioner is obtained, the pH of which is 11.01 and the silicon activation rate is 37.71%.

[0066] The acidic soil conditioner prepared in Example 3 was applied to the acidified soil to be improved at a weight ratio of 0, 0.1%, 0.5%, and 1.5%, and then after cultivation at room temperature, the exchangeable acidity, exchangeable magnesium content, and exchangeable calcium content were measured on the 7th and 28th days, respectively. The soil was stirred irregularly during the cultivation process, and water was replenished every 2 to 3 days to maintain the moisture in the soil at 60% of the maximum field water holding capacity. The relevant data results are recorded in Table 7 below, and the control group is the experimental group when the application of the conditioner is 0, that is, the original acidified soil to be improved (taken from Yuanbao Township, Lichuan City, Enshi, Hubei Province):

[0067] Table 7 Test results of Example 3 before and after improvement by acidic soil conditioner

[0068]

[0069] As can be seen from Table 7, the acidic soil conditioner prepared by the present invention has a good improvement effect on acidified soil. As the amount of the conditioner applied increases, the soil pH value increases accordingly. An application amount of 1.5% can increase the soil pH value from 5.27 to 6.05; secondly, it can effectively reduce the exchangeable acidity of the soil and significantly increase the exchangeable calcium and magnesium content in the soil. It has been found through experiments that the exchangeable calcium and magnesium content is basically stable after 28 days of cultivation. Example 4 A method for preparing an acidic soil conditioner based on phosphogypsum and electrolytic manganese slag, the specific steps are as follows:

[0070] (1) drying the phosphogypsum and electrolytic manganese slag raw materials at 60° C. and then crushing them through a 100-mesh sieve to obtain phosphogypsum powder and electrolytic manganese slag powder;

[0071] (2) placing the dried phosphogypsum powder, electrolytic manganese slag powder, biochar and sodium carbonate obtained in step (1) in a planetary ball mill at a mass ratio of 6:2:1:1, with a ball-to-material ratio of 10:1 and a set speed of 300 r / min, and ball milling for 0.5 h to obtain a silicon activated precursor;

[0072] (3) The silicon activated precursor obtained in step (2) is placed in a crucible and calcined in a muffle furnace from room temperature to 800° C. at a heating rate of 15° C. / min, and calcined at this temperature for 30 min. After crushing, an acidic soil conditioner is obtained, the pH of which is 10.47 and the silicon activation rate is 41.87%.

[0073] The acidic soil conditioner prepared in Example 4 was applied to the acidified soil to be improved at a weight ratio of 0, 0.1%, 0.5%, and 1.5%, and then after cultivation at room temperature, the exchangeable acidity, exchangeable magnesium content, and exchangeable calcium content were measured on the 7th and 28th days, respectively. The soil was stirred irregularly during the cultivation process, and water was replenished every 2 to 3 days to maintain the moisture in the soil at 60% of the maximum field water holding capacity. The relevant data results are recorded in Table 8 below, and the control group is the experimental group when the application of the conditioner is 0, that is, the original acidified soil to be improved (taken from Yuanbao Township, Lichuan City, Enshi, Hubei Province):

[0074] Table 8 Test results of Example 4 before and after improvement by acidic soil conditioner

[0075]

[0076] As can be seen from Table 8, the acidic soil conditioner prepared by the present invention has a good improvement effect on acidified soil. As the application amount of the conditioner increases, the soil pH value increases accordingly. An application amount of 1.5% can increase the soil pH value from 5.27 to 5.77; secondly, it can effectively reduce the exchangeable acidity of the soil and significantly increase the exchangeable calcium and magnesium content in the soil. It was found through experiments that the exchangeable calcium and magnesium contents were basically stable after 28 days of cultivation.

[0077] Based on the above data, biochar has the effect of activating silicon. Comparing Tables 5-8, the modifier in step (3) of Example 2 has the best effect on improving the pH of acidified soil, the modifier in Example 3 increases the exchangeable magnesium content in acidified soil to the maximum, and Example 1 increases the exchangeable calcium content in acidified soil to the maximum. The modifiers in Examples 1-4 can all reduce the exchangeable acidity of acidified soil.

Claims

1. A method for preparing an acidic soil conditioner based on phosphogypsum, comprising the following steps: (1) drying the phosphogypsum raw material at 60°C and then crushing it through a 100-mesh sieve to obtain phosphogypsum powder; (2) placing the dried phosphogypsum powder, biochar and alkali activator obtained in step (1) in a planetary ball mill in a mass ratio of 3:1:1 and fully ball milling to obtain a silicon activated precursor; (3) The activated silicon precursor obtained in step (2) is placed in a muffle furnace and calcined for 0.5-1 h at a calcination temperature of 600-900° C. After cooling, the activated silicon precursor is crushed to obtain an acidic soil conditioner.

2. The preparation method according to claim 1, characterized in that: The ball milling conditions in step (2) are: ball-to-material ratio of 10:1, rotation speed of 300 r / min, and ball milling time of 0.5-1 h.

3. The preparation method according to claim 1, characterized in that: In the step (3), the temperature is raised to 600-900°C at a heating rate of 15°C / min and then calcined for 0.5-1h.

4. The preparation method according to claim 1, characterized in that: The alkaline activator is selected from at least one of calcium hydroxide, sodium hydroxide, sodium sulfate, calcium sulfate, sodium carbonate and water glass.

5. Use of the acidic soil conditioner obtained by the preparation method according to any one of claims 1 to 4 in acidic soil improvement.

6. The use according to claim 5, characterized in that: The specific steps of the application are: mixing the acidic soil conditioner into the acidic soil according to the mass ratio of the acidic soil conditioner to the acidic soil of 0.1% to 5%.