A nickel-based high-temperature alloy powder with high W and Mo content and its application, repair agent and its preparation, and alloy repair method

Through the combination of high W and Mo content nickel-based high-temperature alloy powder and low melting point B-containing activation auxiliary agent, the element ratio is adjusted to form stable W and Mo borides, and the tensile resistance in the high-temperature alloy repair area in the existing technology is solved. The problem of poor performance and antioxidant performance significantly improves the durable performance and antioxidant performance of the repair area and extends the service life of the workpiece.

CN115927917BActive Publication Date: 2024-11-08DONGFANG TURBINE CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202211647242.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-08
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

In the existing powder metallurgical restoration technology, the tensile and oxidation resistance of the high-temperature alloy restoration zone is poor, and the Cr, Mo, W elements combined with B to form large borides and low melting point eutectic phases, resulting in a decrease in joint performance. Moreover, the loss of the Cr, Mo, and W elements causes the performance of the repair zone to deteriorate.

Method used

Use high W and Mo content nickel-based high-temperature alloy powder with low melting point B-containing activation auxiliary agent to adjust the element ratio to form stable W and Mo-rich boronides, avoid the formation of large borides and eutectic phases, and ensure that The element concentration in the repair area is close to the substrate, maintaining the stability of the γ phase and the γ' phase.

Benefits of technology

It significantly improves the durable performance and oxidation resistance of the repair area, extends the service life of the repair workpiece, avoids the loss of Cr, Mo, and W elements, and maintains the mechanical properties and material properties of the repair area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115927917B_ABST
    Figure CN115927917B_ABST
Patent Text Reader

Abstract

The invention discloses a nickel-based high-temperature alloy powder with high W and Mo content, an application thereof, a repairing agent and a preparation thereof, and an alloy repairing method. The alloy powder preparation requires elements and corresponding mass percentages: C (0.05%-0.20%), Cr (15.00%-20.00%), Co (8.00%-12.00%), W (8.00%-12.00%), Mo (10.00%-15.00%), Ta (1.00%-5.00%), Al (4.00%-6.00%), Ti (4.00%-6.00%), and Nb (0-0.60%); the repairing agent comprises alloy powder, a B-containing activation auxiliary agent and a binder, and the alloy powder accounts for 50%-70% of the alloy powder, the B-containing activation auxiliary agent accounts for 25%-45% of the B-containing activation auxiliary agent, and the binder accounts for 5% of the binder. The present invention can stabilize the B element in the low-melting-point B-containing activation auxiliary agent, can effectively weaken the adverse effect of high concentration of B in the repaired joint on the joint performance, significantly improve the durability and oxidation resistance of the repaired area, and can make the metallographic structure characteristics of the repaired area basically consistent with the nickel-based high-temperature alloy casting, thereby ensuring the mechanical properties and material properties of the repaired nickel-based high-temperature alloy casting in the repaired area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of alloy repair materials, in particular to a nickel-based high-temperature alloy powder with high W and Mo content and application thereof, a repair agent and preparation thereof, and an alloy repair method. Background Art

[0002] During the service life of hot-cast and forged parts such as turbine rotor blades and guide vanes of industrial gas turbines, long-term exposure to high temperature and high pressure gas will cause various forms of geometric structural defects such as mechanical fatigue cracks, surface wear, oxidation corrosion and foreign object damage on the surface of the parts. If these defects are not dealt with, they will pose a hidden danger to the safe operation of the unit. Since high-temperature alloys contain a variety of precious metal elements, the production and manufacturing costs are relatively high. If the damaged workpiece is directly replaced, the maintenance cost of the unit will be greatly increased. Repairing the damaged area of ​​the workpiece through effective repair technology can effectively reduce the operation and maintenance costs of the unit. However, as a precipitation-hardened nickel-based high-temperature alloy, high-temperature alloys have poor weldability and the damaged area cannot be repaired by ordinary welding methods.

[0003] Powder metallurgy additive repair is an advanced repair technology for hot-end components of aircraft engines and ground-based combustion engines. It is particularly suitable for the repair and remanufacturing of hot-end components of cast high-temperature alloys with high aluminum and titanium content. The current mainstream repair material is a low-melting point activation auxiliary agent combined with a high-melting point plastic powder. Among them, the composition design of low-melting point activation auxiliary agents, which account for a relatively small proportion, has always been the focus of research. Most of the widely reported and used low-melting point activation auxiliary agents are based on Ni and Co as basic elements, with excessive B added as a melting point reducing element, and appropriate amounts of Ta, Al, Ti, W, Cr, etc. as strengthening elements. For example, commercial grades AMDRYDF-3 (Ni-20Cr-20Co-3Ta-3B-0.02La), NB171 (Ni-10Cr-3.5Si-3.5Fe-2.5B-12W), NB200 (Ni-7Cr-6W-4.5Si-3.2Fe-3.2B-0.06C), AMS4783 (Co-8Si-19Cr-17Ni-4W-0.8B), AMDRYDF-4B (Ni-14Cr-10Co-3.5Al-2.5Ta-2.7B-0.05Y), etc., and some public patents on alloys for structural brazing of superalloy parts, such as CN1056645A, CN1800425A, CN101306494A, CN101780610A, CN101780604A, CN101780612A, CN103894599B, ​​CN109909641A, etc. The high melting point plastic powder, which accounts for a large proportion of the usage, is generally made of high temperature alloy with the same grade as the parent material.

[0004] During the powder metallurgy repair process, the low-melting-point B-containing activation auxiliary agent is first liquefied at high temperature. The B in the liquid phase combines with the Cr, Mo, and W elements in the activation auxiliary agent to form large borides. The remaining B combines with the Cr, Mo, and W elements in the high-melting-point plastic powder. The B content in the liquid phase decreases, the melting point increases, and the repair area solidifies isothermally to form a repaired joint with high strength characteristics. If the Cr, Mo, and W element content in the repair area is not enough to combine all the free B, part of the liquid phase cannot solidify isothermally, and a low-melting-point eutectic will be formed in the repair area when it is cooled. Although the joints repaired by this technology can withstand higher operating temperatures, they still face many problems: First, large borides and low-melting-point eutectic phases are both hard and brittle phases. A large amount of them in the repair area will cause a serious decrease in the tensile properties of the joint. Second, in nickel-based high-temperature alloys, Mo and W are important solid solution strengthening elements of the γ phase, and Cr is one of the most important elements to improve the oxidation resistance and thermal corrosion resistance of the repaired joint. Cr, Mo, and W combine with B in large quantities to form borides, which will cause these elements to lose their original strengthening effect, resulting in a serious decrease in the durability and oxidation resistance of the joint in the repaired area. Third, the concentration of Cr, Mo, and W in the γ phase of the repaired area has dropped seriously. During high-temperature service, the Kirkendall effect will cause the strengthening elements such as Cr, Mo, and W in the parent material to diffuse into the repaired area, resulting in deeper changes in the parent material structure and deterioration of the parent material performance.

[0005] At present, the composition design of repair materials for powder metallurgy additive repair of nickel-based high-temperature alloy castings is mostly concentrated on low-melting-point B-containing activation auxiliary agents with a relatively small usage ratio. There is no targeted composition design for high-melting-point plastic powders with a relatively large usage ratio. Most of them use mature commercial high-temperature alloy powders, which cannot effectively weaken the adverse effects of high concentrations of B in the repaired joints on the joint performance. Summary of the invention

[0006] One purpose of the present invention is: to address the above-mentioned problems, to provide a nickel-based high-temperature alloy powder with high W and Mo content and its application, a repair agent and its preparation, and an alloy repair method, which can stabilize the B element in a low-melting-point B-containing activation auxiliary agent, effectively weaken the adverse effect of high concentration of B in the repaired joint on the joint performance, significantly improve the durability and oxidation resistance of the repaired area, and by adjusting the ratio of the corresponding elements, the metallographic structure characteristics of the repaired area can be made basically consistent with those of the nickel-based high-temperature alloy casting, thereby ensuring the mechanical properties and material properties of the repaired nickel-based high-temperature alloy casting in the repaired area.

[0007] The technical solution adopted by the present invention is as follows: A nickel-based high-temperature alloy powder with high W and Mo content, the preparation of which includes at least the following elements in proportion by mass percentage:

[0008] C (0.05%-0.20%), Cr (15.00%-20.00%), Co (8.00%-12.00%), W (8.00%-12.00%), Mo (10. 00%-15.00%), Ta (1.00%-5.00%), Al (4.00%-6.00%), Ti (4.00%-6.00%), Nb (0-0.60%).

[0009] Further, the remainder is Ni and inevitable impurity elements.

[0010] Furthermore, the contents of Cr, Co, Ta, Al, Ti and Nb in the alloy powder are adjusted according to the composition of the repaired substrate; the contents of Mo and W are adjusted according to the amount of the low-melting-point B-containing activation auxiliary agent and the composition of the repaired substrate.

[0011] Furthermore, the melting temperature of the alloy powder ranges from 1250°C to 1300°C.

[0012] Furthermore, the particle size of the alloy powder is 30 μm-106 μm.

[0013] The alloy powder is used in the repair of nickel-based high-temperature alloys.

[0014] A nickel-based high-temperature alloy repair agent comprises the alloy powder, and also comprises a B-containing activation auxiliary agent and a binder. In terms of mass percentage, the alloy powder accounts for 50%-70%, the B-containing activation auxiliary agent accounts for 25%-45%, and the binder accounts for 5%. The selected binder can be completely volatilized at a temperature below 800°C.

[0015] A method for preparing a nickel-based high-temperature alloy repair agent. To prepare the repair agent, alloy powder and a B-containing activation auxiliary agent are uniformly mixed according to a proportion, and a binder is added to be prepared into a paste.

[0016] A method for repairing a nickel-based high-temperature alloy, using the repair agent, comprises the following steps:

[0017] S1: Pre-treatment of the repair area to make the surface of the repair location clean;

[0018] S2: preparing a repair agent and applying the repair agent to the repair area;

[0019] S3: placing the workpiece in a vacuum environment and heating the workpiece to a temperature of 1190°C-1230°C at a heating rate lower than 16.8°C / min;

[0020] S4: Keep warm for 15-40 minutes and then cool to room temperature with the furnace;

[0021] S5: heating to 1200°C-1210°C in a vacuum environment at a heating rate lower than 10°C / min;

[0022] S6: After keeping warm for 100-200 min, cool to room temperature at a cooling rate greater than 40°C / min.

[0023] Furthermore, the vacuum degree of the vacuum environment is less than 7×10 -3 Pa.

[0024] Furthermore, after step S6, the repaired area is subjected to surface spraying.

[0025] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0026] 1. After the alloy powder disclosed in the present invention is combined with a B-containing activation auxiliary agent to repair the nickel-based high-temperature alloy, the high content of W and Mo in the alloy powder can combine with a large amount of B in the low-melting-point B-containing activation auxiliary agent to form two stable borides, namely, a stable, finely dispersed W-rich boride and a Mo-rich boride, thereby avoiding the loss of Cr in the γ phase, and further avoiding the formation of large borides and eutectic phases, and further achieving that the B in the repair area exists in a form that minimizes damage to the performance of the repair area.

[0027] 2. After the nickel-based high-temperature alloy is repaired using the repair agent disclosed in the present invention, the remaining W, Mo, and Cr contents in the γ phase of the repaired area are close to those of the substrate, and the morphology, size, and precipitation amount of the γ' phase reach the same level as the repaired substrate, ensuring that the repaired area of ​​the nickel-gold high-temperature alloy has excellent oxidation resistance, thermal corrosion resistance, and durability.

[0028] 3. After the nickel-based high-temperature alloy is repaired using the repair agent disclosed in the present invention, the composition of the main elements in the γ and γ' phases in the repaired area is basically consistent with that of the repaired substrate. The Kirkendall effect is weakened during high-temperature service, so that the γ and γ' phases in the repaired substrate remain stable for a long time, thereby extending the service life of the repaired workpiece. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention will now be described by way of example with reference to the accompanying drawings, in which:

[0030] Figure 1 The microscopic morphology of the alloy powder disclosed in the present invention;

[0031] Figure 2 This is the microstructure of the repair area of ​​IN-738LC alloy additively repaired by the repair agent disclosed in Example 3 of the present invention. DETAILED DESCRIPTION

[0032] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0033] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.

[0034] Example 1

[0035] A nickel-based high-temperature alloy powder with high W and Mo content, characterized in that: its preparation includes at least the following elements in proportion by mass percentage:

[0036] C (0.05%-0.20%), Cr (15.00%-20.00%), Co (8.00%-12.00%), W (8.00%-12.00%), Mo (10.00%-15.00%), Ta (1.00%-5.00%), Al (4.00%-6.00%), Ti (4.00%-6.00%), Nb (0-0.60%); the rest is Ni and unavoidable impurity elements.

[0037] The alloy powder in this embodiment has a high content of W and Mo. As a high-melting-point plastic powder, it can be used in combination with a low-melting-point B-containing activation auxiliary agent to repair nickel-based high-temperature alloys. Considering the chemical properties of the B element in the low-melting-point B-containing activation auxiliary agent, the W and Mo in the alloy powder can combine with the B in the low-melting-point B-containing activation auxiliary agent in large quantities to form two stable borides, namely, stable, finely dispersed W-rich borides and Mo-rich borides, thereby avoiding the loss of Cr elements in the γ phase, and further avoiding the formation of large borides and eutectic phases, further achieving the B in the repair area in a form that minimizes damage to the performance of the repair area, and effectively improving the durability and oxidation resistance of the repair area.

[0038] Specifically, C is one of the most important grain boundary strengthening elements in nickel-based high-temperature alloys, and almost all nickel-based high-temperature alloys are added. The C element can be combined with one or more of Cr, Ta, Nb, Mo, W, and Ti to form beneficial carbides (wherein M represents an element or an ionic group) of the types of MC, M6C, M7C3, and M23C6. The carbides are segregated at the grain boundaries, preventing grain boundary sliding and crack formation, thereby facilitating the improvement of the lasting time and lasting plasticity. However, too much carbon addition will cause continuous carbide film layers to be generated on the grain boundaries, making the grain boundaries brittle, easily leading to the nucleation and expansion of cracks, thereby leading to a reduction in the lasting life. Therefore, the content of C is limited to within the range of 0.05wt% to 0.20wt% in the alloy composition of the present invention.

[0039] Cr can improve oxidation resistance and hot corrosion resistance. If the Cr addition is too low, the surface of the repaired area cannot quickly form a continuous and dense Cr2O3 oxide film, resulting in the oxidation resistance and hot corrosion resistance of the repaired area being lower than that of the parent material. If the Cr content is too high, it will promote the precipitation of harmful secondary phases. Therefore, the Cr content in the alloy composition of the present invention is limited to a range of 15.00wt% to 20.00wt%.

[0040] Co can reduce the stacking fault energy of the matrix, making dislocation cross slip difficult, thereby causing solid solution strengthening, and can be infinitely miscible with the nickel-based solid solution. Within a certain range, as the Co content increases, the creep properties of the matrix will be steadily improved. Therefore, the content of Co in the alloy composition of the present invention is limited to the range of 8.00wt% to 12.00wt%.

[0041] The addition amount of Al and Ti directly affects the precipitation amount of the γ' phase in the nickel-based high-temperature alloy, and the precipitation amount of the γ' phase is directly related to the creep performance of the repaired area. In addition, Ti forms MC-type carbides by combining with C, which also helps to improve the strength of the alloy at high temperatures. In the alloy composition of the present invention, the contents of Al and Ti are limited to the range of 4.00wt% to 6.00wt%, which not only ensures the volume fraction of the γ' phase in the repaired area, but also avoids the precipitation and growth of the harmful phase η phase as much as possible.

[0042] The Nb and Ta added to the alloy of the present invention can enter the γ' phase to replace a portion of Al and Ti, change the composition of the γ' phase, inhibit the coarsening of the γ' phase, and improve the stability of the γ' phase, thereby improving the strength and creep resistance of the repaired area. However, too much Nb and Ta addition will cause the repaired area to generate secondary phases such as μ phase and Laves phase that are unfavorable to the performance. Therefore, the content of Nb in the alloy composition of the present invention is limited to the range of 0wt% to 0.60wt%, and the content of Ta is limited to the range of 1.00wt% to 5.00wt%.

[0043] In nickel-based high-temperature alloys, W and Mo are the two main strengthening elements in the γ phase of the nickel-based solid solution, and the solid solution strengthening effect is very significant. However, when the damaged area of ​​the workpiece is repaired by mixing a low-melting-point B-containing activation auxiliary agent with a commercial high-melting-point powder, the B element will combine with the low-content W and Mo in the commercial high-melting-point powder to form borides, causing it to lose all its strengthening effects. Therefore, in the alloy composition of the present invention, the content of W is increased to within the range of 8.00wt% to 12.00wt%, and the content of Mo is increased to within the range of 10.00wt% to 15.00wt%, which is much higher than the addition amount of W and Mo in traditional nickel-based high-temperature alloys. The purpose is to stabilize the B element in the low-melting-point B-containing activation auxiliary agent, and the remaining W and Mo that do not participate in the chemical reaction with B can play a role in solid solution strengthening of the matrix γ phase, thereby solving the problem of poor durability of the repaired joint. Although Cr is also a boride-forming element, the affinity of Cr with B is lower than that of Mo and W, and the boride formed is unstable and easily decomposed at high temperature. Therefore, Cr is not considered as a stabilizing element of boride in the design concept of the present invention. In the alloy composition of the present invention, another beneficial effect of high concentration addition of W and Mo is that a large amount of Cr in the repaired area is avoided from combining with B to cause a large amount of Cr in the γ phase to be consumed, thereby ensuring the oxidation resistance and hot corrosion resistance of the repaired area.

[0044] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting implementation modes are provided. Table 1 shows implementation modes and comparative examples of alloy powders, and the following element content data are all mass percentage data.

[0045] Table 1 Implementation examples and comparative examples of alloy powder (wt%)

[0046]

[0047] It should be noted that the amount and brand of the low melting point B-containing activation auxiliary used in the above examples and the comparative examples are the same, that is, the amount of B element is the same, but the B element in Table 1 is a compound corresponding to the diffusion form. Therefore, there is a difference in the mass percentage and when the WB(n)+MoB(n)+CrB(n) is experimentally determined, but the difference does not affect the summary of the experimental conclusions. The specific conclusions are as follows:

[0048] In this embodiment, when the corresponding alloy powders are used in combination with a low-melting-point B-containing activation auxiliary agent to perform powder metallurgy repair on nickel-based high-temperature parts, the high content of W and Mo in the powder of the present invention can be combined with a large amount of B in the low-melting-point B-containing activation auxiliary agent, and form stable, finely dispersed W-rich borides and Mo-rich borides in the high-melting-point plastic powder, thereby avoiding the loss of Cr in the γ phase and the formation of large borides and eutectic phases. After all the B elements have formed stable borides, the remaining W, Mo, and Cr contents in the γ phase of the repaired area are close to those of the substrate, and the morphology, size, and precipitation amount of the γ' phase are at the same level as those of the repaired substrate, thereby ensuring that the repaired joint has excellent oxidation resistance. Performance, thermal corrosion resistance and durability; For the control examples with grades In738LC, Mar-m247 and GTD111, when the corresponding alloy powders are matched with low-melting-point B-containing activation auxiliary agents for powder metallurgy repair of nickel-based high-temperature parts, the W and Mo contents are low, which are not enough to stabilize the B element in the low-melting-point B-containing activation auxiliary agent, resulting in a large amount of Cr element in the high-melting-point plastic powder being consumed, and the repaired organization contains a large amount of Cr-rich boride and low-melting-point boron-containing eutectic. The W, Mo and Cr contents in the γ phase of the repaired area are much lower than those in the substrate. After heat treatment, the low-melting-point eutectic is melted for the second time to generate holes, and a large amount of B diffuses to the side of the substrate near the weld and combines with W, Mo and Cr to generate borides, resulting in a serious decrease in the W, Mo and Cr contents in the γ phase near the weld side of the substrate, and the organization is seriously damaged. Therefore, the durability, high-temperature oxidation resistance and thermal corrosion resistance of the repaired area obtained by the alloy powder disclosed in the embodiment of the present embodiment are significantly improved.

[0049] As a specific implementation manner, the melting temperature range of the alloy powder is 1250°C-1300°C.

[0050] As a specific implementation method, the particle size of the alloy powder is 30μm-106μm; the particle size is prepared by atomization method; specifically, the high-temperature molten auxiliary agent is atomized by high-pressure water flow, air flow or ultrasonic atomization to form a powder of target particle size, which is conducive to the auxiliary agent being stacked more tightly when repairing the alloy, thereby ensuring the performance of the alloy repair.

[0051] It should be noted that when the alloy powder disclosed in this embodiment is used for repairing nickel-based high-temperature alloys, the contents of Cr, Co, Ta, Al, Ti, and Nb elements in the alloy powder can be adjusted according to the composition of the repaired substrate, and the contents of Mo and W can be adjusted according to the amount of the low-melting-point B-containing activation auxiliary agent and the composition of the repaired substrate; during the repair process, B in the liquid phase is absorbed by the Mo and W added in large quantities in the alloy powder (high-melting-point plastic powder) of this embodiment, and dispersed small-sized granular borides are generated in the high-melting-point plastic powder. Through subsequent heat treatment, Mo, W and other elements in the γ phase of the repair area that have not reacted with B are evenly diffused, so that the content of each solid solution strengthening element in the γ phase of the repair area is basically consistent with that of the repaired substrate, and the morphology, size, and precipitation amount of the γ' phase reach the same level as that of the repaired substrate. During high-temperature service, the element diffusion caused by the Kirkendall effect is weakened, so that the γ and γ' phases of the repaired substrate and the repaired area remain stable for a long time, thereby extending the service life of the repaired workpiece.

[0052] Furthermore, when the alloy powder disclosed in this embodiment is used for the repair of nickel-based high-temperature alloys, the Al+Ti content in the alloy powder is adjusted so that the morphology, size, and precipitation amount of the γ' phase in the repair area can reach the same level as that of the repaired substrate; the W+Mo content in the nickel-based high-temperature alloy powder with high W and Mo content is adjusted according to the addition amount of the low-melting-point B-containing activation auxiliary agent, so as to ensure the content of W, Mo and Cr in the γ phase in the repair area, and effectively improve the durability, high-temperature oxidation resistance and thermal corrosion resistance of the repair area.

[0053] In this embodiment, the alloy powder can be used with a low melting point B-containing activation auxiliary agent to repair various nickel-based cast high-temperature alloys with high aluminum and titanium content, such as IN738LC, Mar-m247, GTD-111, but not limited to the above-mentioned ones.

[0054] It should be noted that the patent "CN111575536" discloses "A nickel-based high-temperature alloy with high W and Mo content", which reduces the degree of internal carbide aggregation and improves the uniformity of the material while ensuring that its conventional mechanical properties are not affected by changing the process manufacturing method, so as to obtain a nickel-based high-temperature alloy with better comprehensive performance. However, the alloy powder proposed in this embodiment is to change the content of its internal constituent elements to ensure the performance of the repair area.

[0055] Example 2

[0056] A nickel-based high-temperature alloy repair agent includes the alloy powder described in Example 1, and also includes a B-containing activation auxiliary agent and a binder. In terms of mass percentage, the alloy powder accounts for 50%-70%, the B-containing activation auxiliary agent accounts for 25%-45%, and the binder accounts for 5%.

[0057] Specifically, taking the repair agent capable of repairing IN-738LC nickel-based high temperature alloy as an example, the alloy powder of the grade DFB-75 in Table 1 of Example 1 is selected, and its microscopic appearance is as follows: Figure 1 The composition of the low melting point B-containing activation auxiliary agent includes the following elements in mass percentage: 10.0% Cr, 10.0% Co, 3.0% Al, 2.0% Ti, 6.0% Ta, 3.0% Re, 3.0% B, and the rest is Ni and unavoidable impurity elements.

[0058] A method for preparing an alloy repair agent. To prepare the alloy repair agent described in this embodiment, a high melting point plastic powder and an auxiliary agent are uniformly mixed according to 30% and 65% by mass respectively, so that equal amounts of high melting point plastic powder and auxiliary agent exist in a unit volume, and a binder with a mass percentage of 5% is added to be prepared into a paste. The paste makes the repair agent viscous and reduces fluidity, so that the repair agent is stable when applied and filled in the repair position, and avoids the repair agent from leaving the repair position before being heated and melted; and the viscous repair agent is more convenient to fill the repair area. Specifically, the viscous state has a certain fluidity. When the repair agent fills the repair position, the repair agent can change its own shape according to the size of the filling position due to its fluidity, so as to meet the filling of irregular repair areas, and can be completely filled under the action of its own fluidity, thereby reducing the defect gaps in the repair area.

[0059] Example 3

[0060] In this embodiment, the method for repairing IN-738LC nickel-based high-temperature alloy using the repair agent described in Example 2 includes the following steps:

[0061] S1: Pre-treatment of the repair area to make the surface of the repair location clean;

[0062] S2: preparing a repair agent and applying the repair agent to the repair area;

[0063] S3: placing the workpiece in a vacuum environment and heating the workpiece to a temperature of 1190°C-1230°C at a heating rate lower than 16.8°C / min;

[0064] S4: Keep warm for 15-40 minutes and then cool to room temperature with the furnace;

[0065] S5: heating to 1200°C-1210°C in a vacuum environment at a heating rate lower than 10°C / min;

[0066] S6: Ensure cooling to room temperature at a cooling rate greater than 40°C / min after 100min-200min.

[0067] Specifically, the defects (repair area) of IN-738LC nickel-based high-temperature alloy with a length, width and height of 40 mm, 3 mm and 2 mm, respectively, are repaired. In step S1, the defects in the repair area are polished clean to prevent impurities from affecting the defect repair; in step S2, the process and method of preparing the repair agent are described in detail in Example 2, and the repair agent is applied to the repair area to complete the additive treatment of the repair area; then, the workpiece is placed in a vacuum heat treatment furnace for additive connection treatment, the heating rate is 10°C / min, the sintering temperature is 1190°C, the insulation is 30 minutes, the vacuum degree is better than 7×10-3 Pa, and the furnace is cooled to room temperature after the insulation is completed; after the workpiece additive connection is completed, it is heated to 1200°C in a vacuum furnace at a heating rate lower than 10°C / min, and after insulation for 120 minutes, it is cooled to room temperature at a cooling rate greater than 40°C / min.

[0068] Furthermore, heating in a vacuum environment can effectively control the gaseous nitrogen element of the material, reducing the content of the gaseous nitrogen element in the material from an average of 300ppm to ≤50ppm, and the vacuum degree of the vacuum environment is less than 7×10 -3 Pa.

[0069] It should be noted that the heating speed is limited by the heating boiler. In order to ensure uniform heating of the workpiece, the heating speed needs to be controlled below 16.8℃ / min. For the choice of insulation time, the insulation time should be sufficient so that the repair agent can completely fill the repair area and evenly expand in the repair area. For the cooling rate, rapid cooling at 40℃ / min can form an excellent γ' phase in the repair area, ensuring the tensile performance, durability and creep performance of the repair area.

[0070] After step S6, the repaired area is subjected to surface spraying to further improve the anti-oxidation ability of the repaired area.

[0071] In this embodiment, the performance test of the defects with length, width and height of 40mm, 3mm and 2mm respectively in IN-738LC nickel-based high-temperature alloy after repair is as follows:

[0072] like Figure 2 As shown, the repair agent affects the microstructure of the repaired area of ​​IN-738LC nickel-based alloy.

[0073] The composition of the γ+γ' phase in the repaired area and inside the substrate grains was measured, as shown in Table 2.

[0074] Table 2 Comparison of the average composition of the γ+γ' phase in the repaired area and the base material grains (wt%)

[0075]

[0076] It can be seen from Table 2 that the chemical compositions of the two tested areas are similar.

[0077] The tensile properties of the repaired joints were measured and the results are shown in Table 3.

[0078] Table 3 Tensile properties of repaired joints

[0079]

[0080] The durability of the repaired joint was measured and the results are shown in Table 4.

[0081] Table 4 Durability of repaired joints

[0082]

[0083] The present invention is not limited to the above-mentioned specific embodiments, but extends to any new features or any new combination disclosed in this specification, as well as any new method or process steps or any new combination disclosed.

Claims

1. A nickel-based high-temperature alloy powder with high W and Mo content, Features: Its preparation includes at least the following elements in proportion by mass percentage: C (0.05%-0.20%), Cr (15.00%-20.00%), Co (8.00%-12.00%), W (8.00%-12.00%), Mo (10.00%-15.00%), Ta (1.00%-5.00%), Al (4.00%-6.00%), Ti (4.00%-6.00%), Nb (0-0.60%); the rest is Ni and unavoidable impurity elements.

2. The nickel-based high-temperature alloy powder with high W and Mo content according to claim 1, Features: The contents of Cr, Co, Ta, Al, Ti and Nb in the alloy powder are adjusted according to the composition of the repaired substrate; the contents of Mo and W are adjusted according to the amount of the low-melting-point B-containing activation auxiliary agent and the composition of the repaired substrate.

3. The nickel-based high-temperature alloy powder with high W and Mo contents according to claim 1, Features: The melting temperature of the alloy powder ranges from 1250°C to 1300°C.

4. The nickel-based high-temperature alloy powder with high W and Mo contents according to claim 1, Features: The particle size of the alloy powder is 30 μm-106 μm.

5. Use of the alloy powder according to any one of claims 1 to 4 in repairing nickel-based high-temperature alloys.

6. A nickel-based high-temperature alloy repair agent, comprising the alloy powder according to any one of claims 1 to 4, Features: It also includes a B-containing activation auxiliary agent and a binder. In terms of mass percentage, the alloy powder accounts for 50%-70%, the B-containing activation auxiliary agent accounts for 25%-45%, and the binder accounts for 5%.

7. A method for preparing a nickel-based high-temperature alloy repair agent, comprising preparing the repair agent according to claim 6, Features: The alloy powder and the B-containing activation auxiliary agent are uniformly mixed according to a certain proportion, and a binder is added to form a paste.

8. A method for repairing a nickel-based high-temperature alloy using the repair agent according to claim 6, Features: The following steps are involved: S1: Pre-treatment of the repair area to make the surface of the repair location clean; S2: preparing a repair agent and applying the repair agent to the repair area; S3: placing the workpiece in a vacuum environment and heating the workpiece to a temperature of 1190°C-1230°C at a heating rate lower than 16.8°C / min; S4: Keep warm for 15-40 minutes and then cool to room temperature with the furnace; S5: heating to 1200°C-1210°C in a vacuum environment at a heating rate lower than 10°C / min; S6: After keeping warm for 100-200 min, cool to room temperature at a cooling rate greater than 40°C / min.

9. The nickel-based high-temperature alloy repair method according to claim 8, Features: The vacuum degree of the vacuum environment is lower than 7×10-3Pa.

10. The nickel-based high-temperature alloy repair method according to claim 8, Features: After step S6, the repaired area is subjected to surface spraying.

Citation Information

Patent Citations

  • Ni-base superalloy solder

    CN101306494A

  • NiCrBSi-NiSiB composite powder brazing material

    CN101780604A

  • NiCoCrWNbMoAlSiBTiC powder brazing material

    CN101780610A

  • NiCoCrWMoNbAlBC foil-shaped brazing material

    CN101780612A

  • A nickel-based powder metallurgy repair material and its application

    CN103894599B