A dental machinable composite material and its preparation method and application

By using a composite material of resin matrix and porous preform in dental restoration materials, combined with freeze casting method and specific resin combination, the deficiencies in mechanical properties and aesthetic properties of existing materials are solved, and high light transmittance and good mechanical properties, simplifying the preparation process and reducing environmental pollution.

CN115944540BActive Publication Date: 2024-10-01AIDITE (QINHUANGDAO) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211589594.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-01
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Existing dental restorative materials have deficiencies in mechanical properties and aesthetic properties, especially the complex preparation process of composite resin materials and the uneven porosity of porous ceramic materials, which limits their application in CAD/CAM systems.

Method used

A composite material of a resin matrix and a porous preform is used. The porous preform is composed of fibers, inorganic powder particles and additives. An ordered lamellar structure is constructed by freeze casting method, combining urethane dimethacrylate and bisphenol A. The use of epoxy resin optimizes the mechanical properties and light transmittance of composite materials.

Benefits of technology

It achieves high light transmittance, good fracture toughness and bending strength, simulates the structure of natural tooth root canals, simplifies the preparation process, reduces production difficulty and environmental pollution, and improves the comprehensive performance of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003991167920000151
    Figure BDA0003991167920000151
Patent Text Reader

Abstract

The present invention provides a dental machinable composite material and a preparation method and application thereof, wherein the machinable composite material comprises two continuous phases, a resin matrix and a porous preform, wherein the raw materials for preparing the porous preform comprise fibers, inorganic powder particles and additives. The structure of the porous preform is an ordered lamellar structure, which not only improves the mechanical properties, but also simulates the structure of the root canal of a natural tooth to a certain extent, and has a certain bionic significance. Compared with a single inorganic powder particle, the addition of fibers to the porous preform not only reduces the defects caused by the lamellar structure, but also prevents the occurrence of cracks to a certain extent. The composite material takes into account the advantages of both inorganic materials and resin materials, combines mechanical properties and aesthetic properties, and has high light transmittance, good fracture toughness and bending strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dental restorative materials, and in particular relates to a dental machinable composite material and a preparation method and application thereof. Background Art

[0002] With the development of the times and the advancement of science and technology, compared with the preparation methods of traditional oral restoration materials, computer-aided design / computer-aided manufacturing (CAD / CAM) methods are widely used in the field of dental restoration. In particular, the emergence of chairside CAD / CAM restoration technology can propose personalized restorations based on the different symptoms of patients, which can meet the needs of patients to a large extent. In addition, chairside CAD / CAM restoration technology is time-saving, fast, accurate, reliable, and has visible effects. It has brought great convenience to both oral patients and dentists and has been increasingly recognized.

[0003] But in contrast, the requirements for machinable dental restoration materials that match the CAD / CAM technology system are getting higher and higher. Dental restoration materials can be divided into metal materials, ceramic materials, resin materials and composite materials according to their composition. Although metal materials have good mechanical properties, their biocompatibility and aesthetic properties are poor. Ceramic materials include all-ceramic materials, feldspar ceramic materials and glass-ceramic materials. Among them, although all-ceramic materials have excellent biocompatibility, aesthetics and mechanical properties, the hardness and modulus of ceramics are much higher than normal teeth, which will cause wear on the opposing teeth, and the complex preparation process limits its use in real life. Although feldspar ceramic materials and glass-ceramic materials have good aesthetic effects, their mechanical properties need to be improved. Although resin materials have low cost and simple preparation process, their mechanical properties are also low, and they are mostly used for temporary restorations.

[0004] Cuttable composite materials generally refer to resin-based composite materials, which can be divided into two categories according to the different preparation processes. One category is based on resin as the matrix, and inorganic particles are mixed and dispersed into the resin matrix to obtain a composite resin, and then high temperature and high pressure are used to cure and shape it; the other category is based on porous ceramics as the matrix, and the resin infiltrates into the porous ceramics. CN112494341A discloses a dental restoration composition and a preparation method thereof, wherein raw materials such as barium glass powder, nano powder, chopped fibers, glass flakes and resin are ball-milled into precursor powder, and dry pressed and heated and pressurized to obtain a composite material suitable for a dental chairside CAD / CAM system. However, this method not only has the problem of uneven powder dispersion, but also the high temperature and high pressure treatment increases the difficulty of actual production. CN106007802A discloses a resin-infiltrated ceramic composite material and a preparation method thereof, wherein a porous ceramic preform is obtained by dry pressing, isostatic pressing and sintering, and then the porous prepolymer is placed in a mixed resin liquid for vacuum impregnation and thermal curing to obtain a resin-infiltrated ceramic composite material. However, this method cannot guarantee the uniformity of the pores in the porous ceramic material. After sintering, some pores may be disconnected, resulting in the porous ceramic material being unable to be completely impregnated with the resin.

[0005] Freeze casting is a method that uses ice crystals as templates and temperature gradients to achieve controllable growth of ice crystals. It is an effective method for preparing oriented ordered porous materials. It has the advantages of low environmental pollution, simple process, controllable porosity, and low processing shrinkage. The ordered porous lamellar structure constructed by freeze casting not only simulates the arrangement structure of dentin tubules, but also has anisotropy. This is a more economical, effective, and simple preparation method than high temperature and high pressure curing of composite resins or dry pressing and sintering of impregnated resins to obtain machinable composite materials. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a dental machinable composite material and a preparation method and application thereof.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a dental machinable composite material, comprising two continuous phases, a resin matrix and a porous preform, wherein the raw materials for preparing the porous preform include fibers, inorganic powder particles and additives.

[0009] The composite material involved in the present invention comprises two continuous phases, a resin matrix and a porous preform, wherein the structure of the porous preform is an ordered lamellar structure, which not only improves the mechanical properties, but also simulates the structure of the root canal of natural teeth to a certain extent, and has a certain bionic significance. Compared with single inorganic powder particles, the addition of fibers in the porous preform not only reduces the defects caused by the lamellar structure, but also prevents the occurrence of cracks to a certain extent. The composite material takes into account the advantages of both inorganic materials and resin materials, combines mechanical properties and aesthetic properties, and has high light transmittance, good fracture toughness and bending strength.

[0010] Preferably, the material of the resin matrix includes any one of bisphenol A-glycidyl dimethacrylate, ethoxylated bisphenol A dimethacrylate, hydroxyethyl methacrylate, carbamate dimethacrylate, triethylene glycol dimethacrylate or bisphenol A epoxy resin, or a combination of at least two thereof; more preferably, it is a combination of carbamate dimethacrylate and bisphenol A epoxy resin.

[0011] The present invention creatively discovers that urethane dimethacrylate and bisphenol A epoxy resin can positively influence each other, and the combined use of the two can improve the mechanical properties and light transmittance of the composite material.

[0012] Preferably, the porosity of the porous preform is 10-50%, for example 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc., and other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one; more preferably, it is 20-30%.

[0013] The porosity of the porous preform is controlled at 10-50%, which is conducive to the penetration of the resin impregnation liquid to form a continuous phase.

[0014] Preferably, the mass ratio of the resin matrix to the porous preform is (1-5):1, for example 1:1, 2:1, 3:1, 4:1, 5:1, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described one by one here.

[0015] When the mass ratio of the resin matrix to the porous preform is (1-5):1, the mechanical properties and light transmittance of the composite material reach the best.

[0016] Preferably, the inorganic powder particles include any one of aluminum oxide, zirconium oxide, calcium hydroxyphosphate, feldspar porcelain powder, barium glass powder, quartz glass powder or sodium aluminum silicate, or a combination of at least two thereof; more preferably, a combination of aluminum oxide and sodium aluminum silicate.

[0017] The present invention creatively discovers that alumina and sodium aluminum silicate have potential interaction, can positively influence each other, and have a certain synergistic effect in improving the mechanical properties and light transmittance of the composite material.

[0018] Preferably, the fiber includes any one of glass fiber, quartz fiber or mullite fiber, or a combination of at least two of them; more preferably, the fiber includes a combination of quartz fiber and mullite fiber.

[0019] The present invention creatively discovers that the combination of quartz fiber and mullite fiber has potential interaction, which can further reduce the defects produced by the lamellar structure, prevent the occurrence of cracks, and improve the mechanical properties of the product.

[0020] Preferably, the mass ratio of the inorganic powder particles and the fibers is (1-5):1, for example 1:1, 2:1, 3:1, 4:1, 5:1, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one.

[0021] Preferably, the additives include a binder and a dispersant.

[0022] Preferably, the binder includes any one of sodium carboxymethyl cellulose, polyvinyl alcohol or chitosan, or a combination of at least two of them.

[0023] Preferably, the dispersant includes any one of citric acid, acetic acid or Dolapix CE 64, or a combination of at least two of them.

[0024] Preferably, the mass of the binder is 1-5% of the mass of the porous preform, such as 1%, 2%, 3%, 4%, 5%, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one.

[0025] Preferably, the mass of the dispersant is 1-10% of the mass of the porous preform, for example 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one.

[0026] In a second aspect, the present invention provides a method for preparing the dental machinable composite material according to the first aspect, the preparation method comprising:

[0027] (1) dispersing fibers, inorganic powder particles and additives in a solvent to obtain a slurry;

[0028] (2) after the slurry is directionally frozen, freeze-dried and sintered to obtain a porous preform;

[0029] (3) subjecting the porous preform to silanization treatment and drying;

[0030] (4) The porous preform after silanization treatment is infiltrated with a resin infiltration liquid, and then thermally cured to obtain the dental machinable composite material.

[0031] The preparation method of the dental machinable composite material involved in the present invention has simple process, easy operation and good repeatability.

[0032] Preferably, the solvent is water and / or tert-butanol.

[0033] Preferably, the dispersion process of the inorganic powder particles, fibers and additives in the solvent is ball milling, the abrasive of the ball milling is zirconia balls, the ball-to-material ratio is (10-20):1, and the time is 2-14h, wherein the specific point values ​​in (10-20) can be selected from 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, etc., and the ball milling time can be selected from 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, etc., and other specific point values ​​within the above numerical ranges can be selected, which will not be repeated here one by one.

[0034] Preferably, the mass ratio of the total mass of the fibers and inorganic powder particles to the solvent is (1-15):20, wherein the specific point values ​​in (1-15) can be selected from 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, etc.

[0035] Preferably, the particle size of the inorganic powder particles is 0.01-20μm, for example, 0.01μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be described one by one here; further preferably, it is 0.01-10μm.

[0036] Preferably, the length of the fiber is 0.1-5mm, for example, 0.1mm, 0.5mm, 1mm, 1.5mm, 2mm, 2.5mm, 3mm, 3.5mm, 4mm, 4.5mm, 5mm, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one; further preferably, it is 1-3mm.

[0037] Preferably, the diameter of the fiber is 0.1-20 μm, for example, 0.1 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc. Other specific point values ​​within the above numerical ranges can be selected, which will not be described one by one here; further preferably, it is 0.5-10 μm,

[0038] Preferably, the ball mill rotation speed is 300-600rpm, for example, 300rpm, 350rpm, 400rpm, 450rpm, 500rpm, 550rpm, 600rpm, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described one by one here.

[0039] Preferably, the temperature of the directional freezing is -180 to -50°C, and the time is 5-10 min. The temperature of the directional freezing can be selected from -180°C, -170°C, -160°C, -150°C, -140°C, -130°C, -120°C, -110°C, -100°C, -90°C, -80°C, -70°C, -60°C, -50°C, etc., and the time of the directional freezing can be selected from 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be repeated here.

[0040] Preferably, the freeze-drying temperature is -60 to -40°C, and the time is 12-24h. The freeze-drying temperature can be selected from -60°C, -55°C, -50°C, -45°C, -40°C, etc., and the freeze-drying time can be selected from 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be repeated here one by one.

[0041] Preferably, the freeze-drying is performed under a vacuum environment.

[0042] Preferably, the heating rate of the sintering treatment is 5-20°C / min, for example, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min, 20°C / min, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be described one by one here.

[0043] Preferably, the temperature of the sintering treatment is 500-800°C, and the time is 10min-2h. The temperature of the sintering treatment can be selected from 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and the time of the sintering treatment can be selected from 10min, 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be repeated here one by one.

[0044] The ordered porous lamellar structure constructed by freeze casting has the advantages of low environmental pollution, simple process, controllable porosity, and small processing shrinkage. It not only simulates the arrangement structure of dentin tubules, but also has anisotropy. It is a more economical, effective and simple preparation method.

[0045] Preferably, the silanization treatment refers to impregnating the porous preform with a silane coupling agent.

[0046] The inorganic component is subjected to surface silanization treatment, which can effectively achieve the bonding between the organic phase and the inorganic phase and reduce the influence of the interface effect.

[0047] Preferably, the impregnation includes vacuum impregnation and normal pressure impregnation.

[0048] Preferably, the silane coupling agent includes any one of γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane or γ-aminopropyltrimethoxysilane, or a combination of at least two thereof;

[0049] Preferably, the silanization treatment temperature is 10-35°C, and the time is 3-6h. The silanization treatment temperature can be selected from 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, etc., and the silanization treatment time can be selected from 3h, 4h, 5h, 6h, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be described one by one here.

[0050] Preferably, the drying temperature is 60-80°C, and the time is 10-20h. The drying temperature can be selected from 60°C, 65°C, 70°C, 75°C, 80°C, etc., and the drying time can be selected from 10h, 12h, 14h, 16h, 18h, 20h, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be described one by one here.

[0051] Preferably, the resin impregnation liquid comprises resin and a curing agent.

[0052] Preferably, the curing agent includes any one of benzoyl peroxide, azobisisobutyronitrile, tert-butyl peracetate or 2-ethyl-4-methylimidazole, or a combination of at least two thereof.

[0053] Preferably, the preparation method of the impregnation liquid is to mix the resin and the curing agent at 55-65°C, for example, 55°C, 57°C, 59°C, 61°C, 63°C, 65°C, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one.

[0054] Preferably, the curing agent is 0.1-2% of the total mass of the resin, for example 0.1%, 0.3%, 0.5%, 0.7%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, etc. Other specific point values ​​within the above numerical ranges can be selected and will not be described here one by one.

[0055] Preferably, the impregnation temperature is 55-65°C, and the time is 1-2h; the impregnation temperature can be selected from 55°C, 57°C, 59°C, 61°C, 63°C, 65°C, and the impregnation time can be selected from 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be repeated here.

[0056] Preferably, the impregnation is performed under vacuum conditions.

[0057] Preferably, the thermal curing temperature is 80-120°C, and the time is 6-20h. The thermal curing temperature can be selected from 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, etc., and the thermal curing time can be selected from 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, etc. Other specific point values ​​within the above numerical ranges can be selected, and they will not be described one by one here.

[0058] In a third aspect, the present invention provides a use of the dental machinable composite material according to the first aspect in preparing a dental restorative material.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] The composite material involved in the present invention comprises two continuous phases, a resin matrix and a porous preform, wherein the structure of the porous preform is an ordered lamellar structure, which not only improves the mechanical properties, but also simulates the structure of the root canal of natural teeth to a certain extent, and has a certain bionic significance. Compared with single inorganic powder particles, the addition of fibers in the porous preform not only reduces the defects caused by the lamellar structure, but also prevents the occurrence of cracks to a certain extent. The composite material takes into account the advantages of both inorganic materials and resin materials, combines mechanical properties and aesthetic properties, and has high light transmittance, good fracture toughness and bending strength.

[0061] The preparation method of the dental machinable composite material involved in the present invention is simple and easy to operate with good repeatability. The ordered porous lamellar structure constructed by the freeze casting method has the advantages of low environmental pollution, simple process, controllable porosity, small processing shrinkage, etc. It not only simulates the arrangement structure of dentin tubules, but also has anisotropy. DETAILED DESCRIPTION

[0062] In order to further explain the technical means and effects adopted by the present invention, the technical solution of the present invention is further described below in conjunction with the preferred embodiments of the present invention, but the present invention is not limited to the scope of the embodiments.

[0063] The sources of the functional ingredients contained in the products involved in the following embodiments, comparative examples, application examples, and comparative application examples are as follows (only the functional ingredients are reflected, and the necessary auxiliary ingredients contained in other commercially available raw materials are not repeated):

[0064] Urethane dimethacrylate was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of diurethane dimethacrylate;

[0065] Bisphenol A epoxy resin was purchased from Sigma under the trade name of Bisphenol A epoxy resin;

[0066] Bisphenol A-glycidyl dimethacrylate was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of glycidyl dimethacrylate;

[0067] Ethoxylated bisphenol A dimethacrylate was obtained from Shanghai Bid Pharmaceutical Technology Co., Ltd. under the trade name of ethoxylated bisphenol A dimethacrylate;

[0068] Hydroxyethyl methacrylate was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of Hydroxyethyl Methacrylate;

[0069] Triethylene glycol dimethacrylate was obtained from a product purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of triethylene glycol dimethacrylate;

[0070] The glass fiber was obtained from a product called glass fiber purchased from Shanghai Puzhen Biotechnology Co., Ltd.

[0071] The quartz fiber was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of quartz fiber;

[0072] The mullite fiber was obtained from a product named Mullite Fiber purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0073] Sodium carboxymethyl cellulose was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name of sodium carboxymethyl cellulose;

[0074] Chitosan was obtained from a product purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. under the trade name Chitosan;

[0075] Polyvinyl alcohol was purchased from Shanghai MacLean Biochemical Co., Ltd. under the trade name of polyvinyl alcohol;

[0076] Dolapix CE 64 is derived from a product purchased from Shanghai Yunguan Electromechanical Equipment Co., Ltd. under the trade name Dolapix CE64 dispersant.

[0077] Example 1

[0078] This embodiment provides a dental machinable composite material, and the preparation method thereof is as follows:

[0079] (1) Preparation of slurry: 20 g of deionized water, acetic acid (5 wt %), 5.5 g of sodium aluminum silicate, 5.5 g of alumina, 1.5 g of quartz fiber, and 1.5 g of mullite fiber were added to a spherical ink tank in sequence, and ball milled at 600 rpm (ball-to-material ratio of 20:1) for 12 h, and then polyvinyl alcohol (2 wt %) was added, and then the speed was reduced and ball milled at 300 rpm for 2 h to obtain a slurry.

[0080] (2) Preparation of porous preform: The slurry was injected into a mold with a copper rod at the bottom, placed in a container filled with liquid nitrogen, and directional frozen at -80°C for 10 min. The frozen sample was placed in a freeze dryer and dried in a vacuum environment at -55°C for 24 h to obtain a porous skeleton. The temperature was raised to 400°C at a rate of 10°C / min, kept at this temperature for 1 h, and then raised to 800°C and kept at this temperature for 10 min to obtain a porous preform.

[0081] (3) Silanization treatment of the porous preform: ethanol, deionized water and γ-methacryloxypropyltrimethoxysilane were mixed in a volume ratio of 80:18:2 to obtain a mixed solution. The porous preform was placed in the mixed solution and vacuum impregnated for 1 hour, keeping other conditions unchanged, and then impregnated at normal pressure for 4 hours, and then dried in a vacuum oven at 60°C for 15 hours.

[0082] (4) Resin infiltration of porous prepolymer: prepare carbamate dimethacrylate and bisphenol A epoxy resin in a mass ratio of 1:1, stir for 3 hours, add benzoyl peroxide (1wt%), and continue stirring for 6 hours to obtain a resin infiltration solution. Immerse the porous preform treated in step (3) in the resin infiltration solution, immerse for 3 hours in a vacuum environment, cure at 80°C for 6 hours, and then cure at 120°C for 6 hours to obtain a dental machinable composite material.

[0083] Example 2

[0084] This embodiment provides a dental machinable composite material, and the preparation method thereof is as follows:

[0085] (1) Preparation of slurry: 20 g of deionized water, citric acid (2 wt%), 5.8 g of zirconium oxide, 5.8 g of calcium hydroxyphosphate, 1.2 g of quartz fiber, and 1.2 g of mullite fiber were added to a ball ink tank in sequence, and ball milled at 600 rpm (ball-to-material ratio of 20:1) for 12 h, and then sodium carboxymethyl cellulose (1 wt%) was added, and then the speed was reduced and ball milled at 300 rpm for 2 h to obtain a slurry.

[0086] (2) Preparation of porous preform: The slurry was injected into a mold with a copper rod at the bottom, placed in a container filled with liquid nitrogen, and directional frozen at -80°C for 10 min. The frozen sample was placed in a freeze dryer and dried in a vacuum environment at -55°C for 20 h to obtain a porous skeleton. The temperature was raised to 400°C at a rate of 10°C / min, kept at this temperature for 1 h, and then raised to 700°C and kept at this temperature for 30 min to obtain a porous preform.

[0087] (3) Silanization treatment of the porous preform: ethanol, deionized water and γ-methacryloxypropyltrimethoxysilane were mixed in a volume ratio of 80:18:2 to obtain a mixed solution. The porous preform was placed in the mixed solution and vacuum impregnated for 1 hour, keeping other conditions unchanged, and then impregnated at normal pressure for 4 hours, and then dried in a vacuum oven at 60°C for 15 hours.

[0088] (4) Resin infiltration of porous prepolymer: Bisphenol A-dimethacrylate glycidyl ester and ethoxylated bisphenol A dimethacrylate were prepared in a mass ratio of 1:1, stirred for 3 hours, and then benzoyl peroxide (1wt%) was added, and the stirring was continued for 6 hours to obtain a resin infiltration solution. The porous preform treated in step (3) was immersed in the resin infiltration solution, immersed in a vacuum environment for 3 hours, and then cured at 80°C for 6 hours, and then cured at 120°C for 6 hours to obtain a dental machinable composite material.

[0089] Example 3

[0090] This embodiment provides a dental machinable composite material, and the preparation method thereof is as follows:

[0091] (1) Preparation of slurry: 20 g of deionized water, Dolapix CE 64 (8 wt %), 4 g of feldspar porcelain powder, 4 g of barium glass powder, 3 g of quartz fiber, and 3 g of glass fiber were added to a ball ink tank in sequence, and ball milled at 600 rpm (ball to material ratio of 20:1) for 12 h, and then chitosan (4 wt %) was added, and then the speed was reduced and ball milled at 300 rpm for 2 h to obtain a slurry.

[0092] (2) Preparation of porous preform: The slurry was injected into a mold with a copper rod at the bottom, placed in a container filled with liquid nitrogen, and directional frozen at -80°C for 10 min. The frozen sample was placed in a freeze dryer and dried in a vacuum environment at -55°C for 20 h to obtain a porous skeleton. The temperature was raised to 400°C at a rate of 10°C / min, kept at this temperature for 1 h, and then raised to 600°C and kept at this temperature for 1 h to obtain a porous preform.

[0093] (3) Silanization treatment of the porous preform: ethanol, deionized water and γ-methacryloxypropyltrimethoxysilane were mixed in a volume ratio of 80:18:2 to obtain a mixed solution. The porous preform was placed in the mixed solution and vacuum impregnated for 1 hour, while keeping other conditions unchanged. After being impregnated at normal pressure for 4 hours, it was taken out and dried in a vacuum oven at 60°C for 15 hours.

[0094] (4) Resin infiltration of porous prepolymer: Hydroxyethyl methacrylate and triethylene glycol dimethacrylate were prepared in a mass ratio of 1:1, stirred for 3 hours, and then benzoyl peroxide (1 wt%) was added, and the stirring was continued for 6 hours to obtain a resin infiltration solution. The porous preform treated in step (3) was immersed in the resin infiltration solution, immersed for 3 hours under a vacuum environment, and cured at 120° C. for 12 hours to obtain a dental machinable composite material.

[0095] Example 4

[0096] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain sodium aluminum silicate, and its mass is distributed to the mass of aluminum oxide, while other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0097] Example 5

[0098] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain aluminum oxide, and its mass is distributed to the mass of sodium aluminum silicate, and other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0099] Example 6

[0100] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain quartz fiber, and its mass is distributed to the mass of mullite fiber, and other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0101] Example 7

[0102] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain mullite fiber, and its mass is distributed to the mass of quartz fiber, and other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0103] Example 8

[0104] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain urethane dimethacrylate, and its mass is allocated to the mass of bisphenol A epoxy resin, while other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0105] Example 9

[0106] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that it does not contain bisphenol A epoxy resin, and its mass is distributed to the mass of urethane dimethacrylate, and other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0107] Example 10

[0108] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that 5.5g of sodium aluminum silicate, 5.5g of aluminum oxide, 1.5g of quartz fiber, and 1.5g of mullite fiber are replaced with 3g of sodium aluminum silicate, 3g of aluminum oxide, 4g of quartz fiber, and 4g of mullite fiber, and the other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0109] Embodiment 11

[0110] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that 5.5g of sodium aluminum silicate, 5.5g of aluminum oxide, 1.5g of quartz fiber, and 1.5g of mullite fiber are replaced with 6g of sodium aluminum silicate, 6g of aluminum oxide, 1g of quartz fiber, and 1g of mullite fiber, and the other components and contents remain unchanged. The preparation method is the same as that of the embodiment 1.

[0111] Example 12

[0112] This embodiment provides a dental machinable composite material, which differs from the embodiment 1 only in that the preparation method of the porous preform is to put the slurry into a steel mold, press at 4 MPa for 2 minutes, heat it to 400°C at a heating rate of 10°C / min after molding, keep it warm for 1 hour, then heat it to 800°C, keep it warm for 10 minutes, and obtain the porous preform. The composition, content and other preparation methods of the composite material remain unchanged.

[0113] Test Example 1

[0114] Test method: According to the standard of GB 30367-2013 dental ceramic materials, the machinable composite material was prepared into a 35mm*4mm*3mm sample, chamfered and polished, and then the flexural strength was tested. There were 10 samples in each group. The machinable composite material was prepared into a 44mm*4mm*3mm sample, polished and V-grooved, and then the fracture toughness was tested. There were 7 samples in each group. The hardness was measured by a Vickers hardness tester (the surface of the 2mm*2mm*2mm sample was smooth), and the light transmittance was measured by a haze meter (circular sample with a diameter of 25mm and a thickness of 1mm).

[0115] Table 1

[0116]

[0117] From the data in Table 1, it can be seen that the dental machinable composite material involved in the present invention has excellent mechanical properties and light transmittance, and meets the standard of GB 30367-2013 dental ceramic materials, and there is a synergistic effect between the urethane dimethacrylate and the bisphenol A epoxy resin in the resin material in improving the mechanical properties and light transmittance of the composite material, there is a synergistic effect between the alumina and the sodium aluminum silicate in the inorganic powder particles in improving the mechanical properties and light transmittance of the composite material, and there is a synergistic effect between the mullite fiber and the quartz fiber in the fiber in improving the mechanical properties of the composite material. In addition, the ordered lamellar structure obtained by directional freezing using the freeze-drying method also has a certain enhancement effect on the mechanical properties and aesthetic properties of the composite material.

[0118] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the dental machinable composite material and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0119] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0120] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A dental machinable composite material, characterized in that: The dental machinable composite material comprises two continuous phases, a resin matrix and a porous preform, wherein the raw materials for preparing the porous preform include fibers, inorganic powder particles and additives; The material of the resin matrix is ​​a combination of urethane dimethacrylate and bisphenol A epoxy resin; The inorganic powder particles are a combination of aluminum oxide and sodium aluminum silicate; The fiber is a combination of quartz fiber and mullite fiber; The mass ratio of the inorganic powder particles to the fibers is (1-5):1; The dental machinable composite material is prepared by the following method, which comprises the following steps: (1) dispersing fibers, inorganic powder particles and additives in a solvent to obtain a slurry; (2) After the slurry is directionally frozen, freeze-dried and sintered to obtain a porous preform; (3) silanizing the porous preform and drying it; (4) The porous preform after silanization treatment is infiltrated with a resin infiltration liquid, and then thermally cured to obtain the dental machinable composite material.

2. The dental machinable composite material according to claim 1, characterized in that: The porosity of the porous preform is 10-50%.

3. The dental machinable composite material according to claim 2, characterized in that: The porosity of the porous preform is 20-30%.

4. The dental machinable composite material according to claim 1, characterized in that: The mass ratio of the resin matrix to the porous preform is (1-5):

1.

5. The dental machinable composite material according to claim 1, characterized in that: The additives include a binder and a dispersant.

6. The dental machinable composite material according to claim 5, characterized in that: The binder includes any one of sodium carboxymethyl cellulose, polyvinyl alcohol or chitosan, or a combination of at least two of them.

7. The dental machinable composite material according to claim 5, characterized in that: The dispersant includes any one of citric acid, acetic acid or Dolapix CE 64 or a combination of at least two of them.

8. The dental machinable composite material according to claim 5, characterized in that: The mass of the binder is 1-5% of the mass of the porous preform.

9. The dental machinable composite material according to claim 5, characterized in that: The mass of the dispersant is 1-10% of the mass of the porous preform.

10. The method for preparing a dental machinable composite material according to any one of claims 1 to 9, characterized in that: The preparation method comprises: (1) dispersing fibers, inorganic powder particles and additives in a solvent to obtain a slurry; (2) After the slurry is directionally frozen, freeze-dried and sintered to obtain a porous preform; (3) silanizing the porous preform and drying it; (4) The porous preform after silanization treatment is infiltrated with a resin infiltration liquid, and then thermally cured to obtain the dental machinable composite material.

11. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The solvent is water and / or tert-butyl alcohol.

12. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The mass ratio of the total mass of the fibers and inorganic powder particles to the solvent is (1-15):

20.

13. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The temperature of the directional freezing is -180~-50°C and the time is 5-10 min.

14. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The freeze-drying temperature is -60~-40°C and the time is 12-24 hours.

15. The method for preparing a dental machinable composite material according to claim 1, characterized in that: The sintering process is carried out at a temperature of 500-800°C and for a time of 10 min-2 h.

16. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The silanization treatment refers to impregnating the porous preform with a silane coupling agent.

17. The method for preparing a dental machinable composite material according to claim 16, characterized in that: The silane coupling agent includes any one of γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane or γ-aminopropyltrimethoxysilane or a combination of at least two thereof.

18. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The temperature of the silanization treatment is 10-35° C. and the time is 3-6 h.

19. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The drying temperature is 60-80°C and the drying time is 10-20 h.

20. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The resin impregnation liquid includes resin and curing agent.

21. The method for preparing a dental machinable composite material according to claim 20, characterized in that: The curing agent includes any one of benzoyl peroxide, azobisisobutyronitrile, tert-butyl peracetate or 2-ethyl-4-methylimidazole, or a combination of at least two thereof.

22. The method for preparing a dental machinable composite material according to claim 20, characterized in that: The mass of the curing agent is 0.1-2% of the total mass of the resin.

23. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The infiltration temperature is 55-65°C and the time is 1-2 h.

24. The method for preparing a dental machinable composite material according to claim 10, characterized in that: The thermal curing temperature is 80-120° C. and the time is 6-20 h.

25. Use of the dental machinable composite material according to any one of claims 1 to 9 in the preparation of dental restorative materials.