Preparation method of rare earth magnesium alloy wire for electric arc additive manufacturing

Through thermal drawing, resistance butt welding and peeling processes, the problems of poor plasticity and uneven performance at the welding during the preparation of rare earth magnesium alloy wire are solved, and efficient and stable wire preparation is achieved, which improves production efficiency and wire material performance.

CN118950733AActive Publication Date: 2024-11-15ZHONGBEI UNIV

Patent Information

Application Number
CN202411103753.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-15
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

When preparing rare earth magnesium alloy wire, due to its poor room temperature plasticity and high temperature deformation resistance, the preparation process is cumbersome and low production efficiency, and there are differences in performance between the welding site and the base material, which is prone to fracture and difficult to achieve high efficiency and stability. silk material preparation.

Method used

Rare earth magnesium alloy wire materials are prepared by thermal drawing, resistance butt welding and peeling processes. Deformation energy storage and defects are reduced through thermal drawing, resistance butt welding relieves stress concentration and tissue differences, peeling removes surface layers, and achieving surface finish and diameter Improved accuracy.

Benefits of technology

It realizes efficient preparation of rare earth magnesium alloy wire with a diameter of Φ1.35~1.45mm without intermediate annealing, which improves the preparation efficiency, ensures the strength of the welding site and the stability of the wire, and avoids breakage. Meets the needs of arc additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950733A_ABST
    Figure CN118950733A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a rare earth magnesium alloy wire suitable for electric arc additive manufacturing, and belongs to the technical field of metal wire machining. The method specifically comprises the following steps that (1) a magnesium alloy bar with the diameter phi of 3-6 mm serves as a raw material, and a wire with the diameter phi of 1.35-1.45 mm is prepared through a hot drawing technology; (2) the wires obtained in the step (1) are connected through a resistance butt welding process; and (3) the wire obtained in the step (2) is subjected to peeling treatment, and finally the magnesium alloy wire with the good surface smoothness and the diameter being # imgabs0 # is obtained. Through the procedures of hot drawing, resistance butt welding and peeling, the length of the obtained wire is not limited, the diameter is uniform, the surface is bright, and peeling and cracks are avoided; meanwhile, the welding head of the resistor pair is compact and free of air holes and oxide inclusions, the strength of the resistor pair is close to that of base metal, and the diameter and roundness of the welding position after peeling treatment are the same as those of a wire; the prepared wire is well matched with a wire feeding system in the subsequent electric arc additive manufacturing process, and the problem of wire breakage is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal wire processing, and in particular relates to a method for preparing a rare earth magnesium alloy wire for arc additive manufacturing. Background Art

[0002] Rare earth magnesium alloys have broad application prospects in aerospace, transportation, weapons and equipment due to their low density, high specific strength and stiffness, and good high temperature performance. In particular, magnesium alloys have incomparable advantages in replacing traditional steel materials and significantly reducing the weight of structures such as missiles and satellites. Since magnesium has a close-packed hexagonal structure, the number of glide system actuations at room temperature is small, and the plastic deformation capacity is poor, traditional processing methods face many challenges. Arc additive manufacturing technology uses arc as a heat source and metal wire as a raw material. By precisely controlling parameters and stacking layers, it can achieve efficient preparation of large-size and complex-shaped structures, thus providing new technical support for the development and preparation of rare earth magnesium alloy products.

[0003] The wire diameter used in arc additive manufacturing is usually Φ1.2mm. For rare earth magnesium alloys, wire preparation is very difficult due to poor room temperature plasticity and high resistance to high temperature deformation. Specifically, (1) frequent drawing and annealing make the process cumbersome and the production efficiency is low; (2) breakage is easy to occur during the drawing process, and the machine needs to be shut down and restarted, which reduces production efficiency, and the length of the prepared wire is limited; (3) Although thick wires can be welded to increase their length, there are still differences in microstructure and performance between the weld and the parent material, and wire breakage will still occur during the subsequent frequent drawing and annealing process. Therefore, efficient rare earth magnesium alloy wire preparation methods and high-quality rare earth magnesium alloy wire raw materials have become one of the current research hotspots. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing rare earth magnesium alloy wire for arc additive manufacturing, which is prepared by hot drawing, resistance welding and peeling process. Magnesium alloy wire can achieve the preparation of rare earth magnesium alloy wire for arc additive manufacturing with good surface finish and stable and reliable performance.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing rare earth magnesium alloy wire for arc additive manufacturing, using magnesium alloy rods with a diameter of Φ3 to 6 mm as raw materials, and preparing a magnesium alloy wire with a diameter of Φ3 to 6 mm by hot drawing, resistance butt welding and peeling processes. The magnesium alloy wire material, the preparation method comprises the following steps:

[0007] Step 1: hot drawing forming: the magnesium alloy rod is pulled by a drawing reel and sequentially passes through a lubricant, a tubular heating furnace and a drawing die to achieve the purpose of reducing the diameter. After several hot drawing passes, a wire with a diameter of Φ1.35-1.45 mm is prepared;

[0008] Step 2: resistance butt welding. The end face of the wire obtained in step 1 is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. Under argon protection, power is turned on. The end faces of the wires are connected through preheating, welding and slow cooling. Finally, the butt welding joint is polished and smooth.

[0009] Step 3: peeling. The wire obtained in step 2 is pulled by the peeling machine drum through a peeling die or a peeling die and a calendering die to remove the lubricating layer and oxide layer on the surface of the wire and control the diameter accuracy of the finished wire. The last peeling is performed by a combination of a peeling die and a calendering die to obtain a wire with a good surface finish and a diameter of Magnesium alloy wire.

[0010] Furthermore, the composition of the magnesium alloy rod comprises, by mass percentage, 8-13% Gd, 0-5% Y, 0-3% Zn, 0-0.3% Zr, and the remainder is Mg.

[0011] Furthermore, in the step 1, a reel with a diameter of Φ800 mm is used for hot drawing of magnesium alloy rods with a diameter of Φ3-6 mm, and a reel with a diameter of Φ400 mm is used for hot drawing of magnesium alloy wires with a diameter of less than 3 mm.

[0012] Furthermore, in step 1, the lubricant used in the hot drawing is graphite emulsion, the hot drawing temperature is 400-500° C., the hot drawing single-mode deformation is 10%-20%, and the hot drawing rate is 1-3 m / min.

[0013] Furthermore, in the step 2, the spacing between the resistance butt welding fixtures is 1 to 3 mm, and the end faces are ensured to be strictly aligned, the preheating current is 50 to 80 A, the time is 0.05 to 0.1 s, and the top forging pressure is 0.02 to 0.06 MPa, the welding current is 100 to 200 A, the time is 0.3 to 0.6 s, and the top forging pressure is 0.1 to 0.3 MPa, the slow cooling current is 10 to 40 A, the time is 0.1 to 0.2 s, and the top forging pressure is 0 MPa.

[0014] Further, in the step three, the diameter of the reel used for peeling is Φ400mm; wherein, the first and second peeling passes only use a peeling die, the diameter reduction of a single die is 0.1-0.2mm, the peeling rate is 10-20m / min, and a magnesium alloy wire with a diameter of Φ1.25mm is obtained; the last peeling pass uses a combination die of a peeling die and a calendering die, and the corresponding peeling die diameter reduction is 0.03mm, the calendering die diameter reduction is 0.02mm, the peeling rate is 10m / min, and a magnesium alloy wire with a diameter of Φ1.25mm is obtained. Magnesium alloy wire.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The present invention adopts a single-mode hot drawing forming process, and the rod / wire is heated to a relatively high temperature before being deformed by the mold, which not only eliminates the deformation energy storage and defects caused by the previous deformation to a certain extent, but also greatly reduces the deformation energy storage and defects caused by this deformation, avoiding the accumulation of deformation energy storage and defects. Therefore, the wire preparation technology disclosed in the present invention makes full use of the basic principle of thermal deformation, and reasonably matches the relationship between deformation temperature, single-mode deformation and drawing rate under good lubrication conditions, realizing the preparation process of rare earth magnesium alloy wire from Φ6mm to Φ1.35~1.45mm without the need for an intermediate annealing process, shortening the preparation process and improving the preparation efficiency.

[0017] 2. The present invention adopts the resistance welding process to connect the wires. The end face of the wire undergoes the process of preheating, welding and slow cooling, which greatly alleviates the stress concentration caused by direct welding and the difference between the weld and the parent material structure. Under the action of the top forging pressure, the weld presents the characteristics of dense, pore-free and oxide-free structure. At the same time, the strength of the weld can be close to that of the parent material without intermediate annealing, thereby ensuring that the weld will not break during the subsequent stripping process and the wire feeding process of arc additive manufacturing. Therefore, the resistance welding technology disclosed in the present invention combines the traditional resistance welding technology with the heat treatment technology through automatic control, and realizes the efficient, high-performance and stable connection of the wire.

[0018] 3. The present invention adopts a peeling process to remove the lubricating layer and the oxide layer on the surface of the wire, and adopts a combined die consisting of a peeling die and a calendering die in the last peeling process to further remove the micro grooves formed on the surface of the wire by the previous peeling process, thereby improving the surface finish of the wire and controlling the accuracy of the diameter of the finished wire to achieve In summary, the peeling process disclosed in the present invention can simultaneously achieve the effects of reducing the diameter of the wire, improving the surface finish and improving the diameter accuracy.

[0019] 4. The present invention adopts the process of hot drawing-resistance welding-stripping to produce rare earth magnesium alloy wire for arc additive. After the hot-drawn wire is subjected to resistance welding, the wire of any length can be prepared; after the welding part is simply polished and smoothed, the diameter reduction of the stripping die is controlled to ensure that the welding part is not broken, and the rare earth magnesium alloy wire with uniform and stable diameter, unlimited length and good surface finish can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a photograph of the second phase morphology in the rare earth magnesium alloy wire with a diameter of Φ1.4 mm prepared by hot drawing in Example 1 of the present invention.

[0021] Figure 2 This is a photograph of the grain morphology of the rare earth magnesium alloy wire with a diameter of Φ1.4 mm prepared by hot drawing in Example 1 of the present invention.

[0022] Figure 3 This is the room temperature tensile stress-strain curve of the rare earth magnesium alloy wire with a diameter of Φ1.4 mm prepared by hot drawing in Example 1 of the present invention.

[0023] Figure 4 This is a microstructure photograph of the weld after resistance butt welding of rare earth magnesium alloy wire with a diameter of Φ1.4 mm in Example 1 of the present invention.

[0024] Figure 5 This is the room temperature tensile stress-strain curve of the rare earth magnesium alloy wire with a diameter of Φ1.4 mm after resistance butt welding in Example 1 of the present invention.

[0025] Figure 6 The diameter of the peeled sample is Macro photo of rare earth magnesium alloy wire.

[0026] Figure 7 The diameter of the peeled sample is Surface micromorphology of rare earth magnesium alloy wire. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a rare earth magnesium alloy wire for arc additive manufacturing, which uses a magnesium alloy rod with a diameter of Φ3 to 6 mm as a raw material (the preparation of a magnesium alloy rod with a diameter of Φ3 to 6 mm is a prior art, for example, it can be prepared by the staged deformation hot extrusion technology described in CN2024100464283, which will not be repeated here), and the specific composition includes the following mass percentages: 8-13% Gd, 0-5% Y, 0-3% Zn, 0-0.3% Zr, and the rest is Mg; the magnesium alloy rod is prepared by hot drawing, resistance butt welding and peeling process to obtain a magnesium alloy wire with a diameter of Φ3 to 6 mm. The magnesium alloy wire comprises the following steps:

[0028] Step 1, hot drawing forming, the magnesium alloy rod is pulled by the drawing reel and sequentially passes through the lubricant, tubular heating furnace and drawing die to achieve the purpose of reducing the diameter, and a wire with a diameter of Φ1.35-1.45mm is prepared after several passes of hot drawing. As a specific implementation method, a reel with a diameter of Φ800mm is used for hot drawing of magnesium alloy rod raw materials with a diameter of Φ3-6mm. During the hot drawing process, a reel with a diameter of Φ400mm is used for hot drawing of magnesium alloy wires with a diameter of less than 3mm. As the diameter decreases, the residual stress generated by deformation and cooling can easily lead to an increase in the bending degree of the wire, and even entanglement, so that the wire release process cannot proceed normally, so a small reel is used to adapt to the bending degree of the wire and improve the neatness of the entire coil of wire. In addition, the lubricant used for hot drawing of the present invention is graphite emulsion, the hot drawing temperature is 400-500℃, the hot drawing single mode deformation is 10%-20%, and the hot drawing rate is 1-3m / min. In the conventional drawing + intermediate annealing process, intermediate annealing is used to eliminate the deformation energy storage and defects caused by deformation. However, if the intermediate annealing is not thorough, the plastic deformation ability of the wire cannot be restored, and continued deformation is very likely to lead to fracture; excessive intermediate annealing will cause abnormal growth of both the grains and the second phase in the alloy, which will lead to uneven microstructure and poor plastic deformation ability of the material. This step makes full use of the basic principle of thermal deformation. Under good lubrication conditions, the relationship between deformation temperature, single-mode deformation and drawing rate is reasonably matched, so that the wire can always maintain good and stable plastic deformation ability, and realize the preparation of rare earth magnesium alloy wire with a diameter of Φ6mm to Φ1.35~1.45mm without the need for intermediate annealing.

[0029] Step 2: resistance butt welding. The end face of the wire obtained in step 1 is polished and smoothed. At the same time, the lubricating layer and oxide layer on the surface of the wire within 10mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed to the fixture of the resistance butt welding machine. Under argon protection, power is turned on. The end faces of the wires undergo preheating, welding and slow cooling processes to achieve connection. Finally, the butt welding joint is polished and smooth. In this step, the spacing between the resistance butt welding fixtures is 1 to 3mm, and the end faces are strictly aligned. The preheating current is 50 to 80A, the time is 0.05 to 0.1s, and the forging pressure is 0.02 to 0.06MPa. The welding current is 100 to 200A, the time is 0.3 to 0.6s, and the forging pressure is 0.1 to 0.3MPa. The slow cooling current is 10 to 40A, the time is 0.1 to 0.2s, and the forging pressure is 0MPa. The present invention adopts the resistance welding process to connect the wires. The end face of the wire undergoes the process of preheating, welding and slow cooling, which greatly alleviates the stress concentration caused by direct welding and the difference between the weld and the parent material structure. Under the action of the top forging pressure, the weld presents the structure characteristics of dense, pore-free and oxide-free inclusions. At the same time, the strength of the weld can be close to that of the parent material without intermediate annealing, thereby ensuring that the weld does not break during the subsequent peeling process and the wire feeding process of arc additive manufacturing. The inventor believes that it is effective to use the above parameters during the above preheating, welding and cooling. For the preheating, welding and slow cooling process, if the temperature is higher than the parameter range, the temperature of the wire end face will be too high and the cooling will not be timely, which will lead to serious surface oxidation, inclusions, poor end face bonding, and coarse grains and second phases at the weld; if the temperature is lower than the parameter range, the temperature of the wire end face will be too low, which will lead to incomplete end face welding and excessive residual stress at the weld. Therefore, the above parameters of preheating, welding and slow cooling are effective.

[0030] Step 3: peeling. The wire obtained in step 2 is pulled by the peeling machine drum through a peeling die or a peeling die and a calendering die to remove the lubricating layer and oxide layer on the surface of the wire and control the diameter accuracy of the finished wire. The last peeling is performed by a combination of a peeling die and a calendering die to obtain a wire with a good surface finish and a diameter of In this step, the diameter of the reel used for peeling is Φ400mm; in the first and second peeling passes, only the peeling die is used, the diameter reduction of the single die is 0.1-0.2mm, the peeling rate is 10-20m / min, and the magnesium alloy wire with a diameter of Φ1.25mm is obtained; the last peeling pass uses a combination of a peeling die and a calendering die, and the corresponding peeling die diameter reduction is 0.03mm, the calendering die diameter reduction is 0.02mm, and the peeling rate is 10m / min, and the diameter is obtained. The peeling process simultaneously achieves the effect of wire diameter reduction, improved surface finish and improved diameter accuracy.

[0031] The present invention will further explain in detail a method for preparing a rare earth magnesium alloy wire for arc additive manufacturing through the accompanying drawings and specific embodiments. It should be pointed out that these specific embodiments are only used to illustrate the present invention and do not constitute any limitation to the present invention.

[0032] Example 1

[0033] This embodiment provides a method for preparing Mg-9Gd-4Y-1Zn-0.3Zr (wt%) alloy wire for arc additive manufacturing. The diameter of the magnesium alloy rod raw material is Φ5mm. The method specifically includes the following steps:

[0034] Step 1: hot drawing forming. The rare earth magnesium alloy rod / wire is pulled by a drawing reel and sequentially passes through a lubricant, a tubular heating furnace and a drawing die to achieve the purpose of reducing the diameter. During the hot drawing process, a reel with a diameter of Φ800mm is used for hot drawing of magnesium alloy rods / wires with a diameter of Φ5-3mm, and a reel with a diameter of Φ400mm is used for hot drawing of magnesium alloy rods / wires with a diameter of less than Φ3mm. The lubricant used for hot drawing is graphite emulsion, the hot drawing temperature is 450°C, the hot drawing single-mode deformation is 15%, and the hot drawing rate is 2.5m / min. After 16 hot drawing passes, a wire with a diameter of Φ1.4mm is prepared;

[0035] Step 2: resistance butt welding. The end face of the wire obtained in step (1) is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. The distance between the fixtures is 2 mm. The end faces are ensured to be strictly aligned. The power is turned on under argon protection. The end faces of the wire are connected through preheating, welding and slow cooling. The preheating current is 50A, the time is 0.1s, and the forging pressure is 0.05MPa. The welding current is 180A, the time is 0.4s, and the forging pressure is 0.2MPa. The slow cooling current is 10A, the time is 0.2s, and the forging pressure is 0MPa. Finally, the butt welding joint is polished and smooth.

[0036] Step 3: peeling. The wire obtained in step (2) is pulled by a peeling machine drum through a peeling die and a combined die including a peeling die and a calendering die, wherein the drum diameter is Φ400 mm, the diameter reduction of the peeling die in one pass is 0.15 mm, and the peeling rate is 20 m / min, so as to obtain a magnesium alloy wire with a diameter of Φ1.25 mm; in the combined die of the peeling die and the calendering die, the diameter reduction of the peeling die is 0.03 mm, the diameter reduction of the calendering die is 0.02 mm, and the peeling rate is 10 m / min, so as to obtain a magnesium alloy wire with a diameter of Magnesium alloy wire.

[0037] The microstructure and room temperature tensile stress-strain curve of the Mg-9Gd-4Y-1Zn-0.3Zr alloy wire with a diameter of Φ1.4 mm prepared by hot drawing in this embodiment are shown in Figure 1 , 2 As shown in Figure 3 and Figure 4. From the characterization of the microstructure, it can be seen that there are a large number of strip-shaped and granular second phases inside the wire, and most of the granular sizes are less than 5μm, and the average grain size is about 8μm. Therefore, after hot drawing deformation, the second phase and grain size in the alloy are significantly refined. The room temperature tensile test shows that the wire yield strength reaches 280MPa, the tensile strength reaches 330MPa, and the elongation reaches 9%. The microstructure and room temperature tensile stress-strain curve of the weld after resistance butt welding are shown in Figure 4. Figure 4 and 5 As shown. It can be seen that a discontinuous network of second phases is formed at the grain boundaries at the weld, and the grain size is about 1μm; there is a heat-affected zone between the weld and the base material, which serves as a transition zone for microstructural changes. During the room temperature tensile test, the specimen broke in the heat-affected zone, and the yield strength reached 283MPa, the tensile strength reached 315MPa, and the elongation reached 4%. It can be seen that the strength of the weld after resistance butt welding is close to that of the base material, and the plasticity is greatly reduced compared to the base material, but the high strength and low plasticity matching can still ensure smooth wire feeding during the arc additive process. The diameter after peeling is The macroscopic photos and surface microscopic morphology of the wire are shown in Figure 6 and 7 As shown in the figure, the surface of the wire is bright, without peeling or cracks, and the diameter is concentrated between Φ1.19 and 1.20 mm, which can meet the requirements of dimensional accuracy; at the same time, the surface is microscopic, and no microgrooves caused by the peeling mold are observed in the microscopic morphology. A large number of fine second phase particles are observed to be distributed on the surface, which further shows that the surface finish of the wire is good.

[0038] Example 2

[0039] This embodiment provides a method for preparing Mg-8Gd-3Y-2Zn-0.3Zr (wt%) alloy wire for arc additive manufacturing. The diameter of the magnesium alloy rod raw material is Φ6mm. The method specifically includes the following steps:

[0040] Step 1: hot drawing forming. The rare earth magnesium alloy rod / wire is pulled by a drawing reel and sequentially passes through a lubricant, a tubular heating furnace and a drawing die to achieve the purpose of reducing the diameter. During the hot drawing process, a reel with a diameter of Φ800mm is used for hot drawing of magnesium alloy rods / wires with a diameter of Φ6-3mm, and a reel with a diameter of Φ400mm is used for hot drawing of magnesium alloy rods / wires with a diameter of less than Φ3mm. The lubricant used for hot drawing is graphite emulsion, the hot drawing temperature is 500℃, the hot drawing single-mode deformation is 20%, and the hot drawing rate is 1m / min. After 14 hot drawing passes, a wire with a diameter of Φ1.35mm is prepared;

[0041] Step 2: resistance butt welding. The end face of the wire obtained in step (1) is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. The distance between the fixtures is 1 mm. Ensure that the end faces are strictly aligned. Power is turned on under argon protection conditions. The end faces of the wires are connected through preheating, welding and slow cooling processes. The preheating current is 80A, the time is 0.05s, and the forging pressure is 0.02MPa. The welding current is 200A, the time is 0.3s, and the forging pressure is 0.1MPa. The slow cooling current is 40A, the time is 0.1s, and the forging pressure is 0MPa. Finally, the butt welding joint is polished and smooth.

[0042] Step 3: peeling. The wire obtained in step (2) is pulled by a peeling machine drum through a peeling die and a combined die including a peeling die and a calendering die, wherein the drum diameter is Φ400 mm, the diameter reduction of the peeling die in one pass is 0.1 mm, and the peeling rate is 15 m / min, so as to obtain a magnesium alloy wire with a diameter of Φ1.25 mm; in the combined die of the peeling die and the calendering die, the diameter reduction of the peeling die is 0.03 mm, the diameter reduction of the calendering die is 0.02 mm, and the peeling rate is 10 m / min, so as to obtain a magnesium alloy wire with a diameter of Magnesium alloy wire.

[0043] In this embodiment, a Mg-8Gd-3Y-2Zn-0.3Zr alloy wire with a diameter of Φ1.35 mm was prepared by hot drawing. The room temperature tensile test showed that the wire yield strength reached 260 MPa, the tensile strength reached 350 MPa, and the elongation reached 5%. After resistance butt welding, the sample broke in the heat affected zone during the room temperature tensile test, and the yield strength reached 266 MPa, the tensile strength reached 340 MPa, and the elongation reached 3.7%.

[0044] Example 3

[0045] This embodiment provides a method for preparing Mg-8Gd-3Y-0.3Zr (wt%) alloy wire for arc additive manufacturing. The diameter of the magnesium alloy rod raw material is Φ3mm. The method specifically includes the following steps:

[0046] Step 1: hot drawing. The rare earth magnesium alloy rod / wire is pulled by a drawing reel and passes through a lubricant, a tubular heating furnace and a drawing die in sequence to achieve the purpose of reducing the diameter. During the hot drawing process, a reel with a diameter of Φ400mm is used for hot drawing of magnesium alloy rods / wires with a diameter less than Φ3mm. The lubricant used for hot drawing is graphite emulsion. The hot drawing temperature is 400℃, the hot drawing single-mode deformation is 10%, and the hot drawing rate is 3m / min. After 14 hot drawing passes, a wire with a diameter of Φ1.45mm is prepared;

[0047] Step 2: resistance butt welding. The end face of the wire obtained in step (1) is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. The distance between the fixtures is 3 mm. The end faces are ensured to be strictly aligned. The power is turned on under argon protection. The end faces of the wire are connected through preheating, welding and slow cooling. The preheating current is 60A, the time is 0.08s, and the forging pressure is 0.06MPa. The welding current is 100A, the time is 0.6s, and the forging pressure is 0.3MPa. The slow cooling current is 20A, the time is 0.15s, and the forging pressure is 0MPa. Finally, the butt welding joint is polished and smooth.

[0048] Step 3: peeling. The wire obtained in step (2) is pulled by a peeling machine drum through a peeling die and a combined die including a peeling die and a calendering die, wherein the drum diameter is Φ400 mm, the diameter reduction of the peeling die in one pass is 0.2 mm, and the peeling rate is 10 m / min, so as to obtain a magnesium alloy wire with a diameter of Φ1.25 mm; in the combined die of the peeling die and the calendering die, the diameter reduction of the peeling die is 0.03 mm, the diameter reduction of the calendering die is 0.02 mm, and the peeling rate is 10 m / min, so as to obtain a magnesium alloy wire with a diameter of Magnesium alloy wire.

[0049] In this embodiment, a Mg-8Gd-3Y-0.3Zr alloy wire with a diameter of Φ1.45 mm was prepared by hot drawing. The room temperature tensile test showed that the wire had a yield strength of 370 MPa, a tensile strength of 420 MPa, and an elongation of 4.7%. After resistance butt welding, the sample broke in the heat-affected zone during the room temperature tensile test, and the yield strength reached 383 MPa, the tensile strength reached 400 MPa, and the elongation reached 3.5%.

[0050] Example 4

[0051] This embodiment provides a method for preparing Mg-13Gd-1Zn (wt%) alloy wire for arc additive manufacturing, wherein the diameter of the magnesium alloy rod raw material is Φ5mm. Specifically, the following steps are included:

[0052] Step 1: hot drawing forming. The rare earth magnesium alloy rod / wire is pulled by a drawing reel and sequentially passes through a lubricant, a tubular heating furnace and a drawing die to achieve the purpose of reducing the diameter. During the hot drawing process, a reel with a diameter of Φ800mm is used for hot drawing of magnesium alloy rods / wires with a diameter of Φ5 to 3mm, and a reel with a diameter of Φ400mm is used for hot drawing of magnesium alloy rods / wires with a diameter less than Φ3mm. The lubricant used for hot drawing is graphite emulsion, the hot drawing temperature is 450°C, the hot drawing single-mode deformation is 15%, and the hot drawing rate is 2m / min. After 16 hot drawing passes, a wire with a diameter of Φ1.45mm is prepared;

[0053] Step 2: resistance butt welding. The end face of the wire obtained in step (1) is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. The distance between the fixtures is 2 mm. The end faces are ensured to be strictly aligned. The power is turned on under argon protection. The end faces of the wire are connected through preheating, welding and slow cooling. The preheating current is 80A, the time is 0.08s, and the forging pressure is 0.05MPa. The welding current is 150A, the time is 0.4s, and the forging pressure is 0.2MPa. The slow cooling current is 20A, the time is 0.2s, and the forging pressure is 0MPa. Finally, the butt welding joint is polished and smooth.

[0054] Step 3: peeling. The wire obtained in step (2) is pulled by a peeling machine drum through two peeling dies and one combined die including a peeling die and a calendering die, wherein the drum diameter is Φ400 mm, the diameter reduction of the peeling die in 1 to 2 passes is 0.1 mm, and the peeling rate is 20 m / min, so as to obtain a magnesium alloy wire with a diameter of Φ1.25 mm; in the combined die of the peeling die and the calendering die, the diameter reduction of the peeling die is 0.03 mm, the diameter reduction of the calendering die is 0.02 mm, and the peeling rate is 10 m / min, so as to obtain a magnesium alloy wire with a diameter of Magnesium alloy wire.

[0055] In this embodiment, a Mg-13Gd-1Zn alloy wire with a diameter of Φ1.45 mm was prepared by hot drawing. The room temperature tensile test showed that the wire had a yield strength of 496 MPa, a tensile strength of 553 MPa, and an elongation of 4%. After resistance butt welding, the sample broke in the heat-affected zone during the room temperature tensile test, and the yield strength reached 455 MPa, the tensile strength reached 480 MPa, and the elongation reached 4.2%.

[0056] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing rare earth magnesium alloy wire for arc additive manufacturing, characterized in that: The preparation method uses magnesium alloy rods with a diameter of Φ3 to 6 mm as raw materials, and prepares magnesium alloy rods with a diameter of Φ3 to 6 mm through hot drawing, resistance butt welding and peeling processes. The magnesium alloy wire material, the preparation method comprises the following steps: Step 1: hot drawing forming: the magnesium alloy rod is pulled by a drawing reel and sequentially passes through a lubricant, a tubular heating furnace and a drawing die to achieve the purpose of reducing the diameter. After several hot drawing passes, a wire with a diameter of Φ1.35-1.45 mm is prepared; Step 2: resistance butt welding. The end face of the wire obtained in step 1 is polished and smoothed. At the same time, the lubricating layer and the oxide layer on the surface of the wire within 10 mm on one side of the end face are polished and cleaned. The end faces of the two sections of wire are aligned and fixed on the fixture of the resistance butt welding machine. Under argon protection, power is turned on. The end faces of the wires are connected through preheating, welding and slow cooling. Finally, the butt welding joint is polished and smooth. Step 3: peeling. The wire obtained in step 2 is pulled by the peeling machine drum through a peeling die or a peeling die and a calendering die to remove the lubricating layer and oxide layer on the surface of the wire and control the diameter accuracy of the finished wire. The last peeling is performed by a combination of a peeling die and a calendering die to obtain a wire with a good surface finish and a diameter of Magnesium alloy wire.

2. The method for preparing rare earth magnesium alloy wire for arc additive manufacturing according to claim 1, characterized in that: The composition of the magnesium alloy rod comprises, by mass percentage, 8-13% Gd, 0-5% Y, 0-3% Zn, 0-0.3% Zr, and the rest is Mg.

3. The method for preparing rare earth magnesium alloy wire for arc additive manufacturing according to claim 1, characterized in that: In the step 1, a reel with a diameter of Φ800 mm is used for hot drawing of magnesium alloy rods with a diameter of Φ3-6 mm, and a reel with a diameter of Φ400 mm is used for hot drawing of magnesium alloy wires with a diameter of less than 3 mm.

4. The method for preparing rare earth magnesium alloy wire for arc additive manufacturing according to claim 1, characterized in that: In the step 1, the lubricant used in the hot drawing is graphite emulsion, the hot drawing temperature is 400-500° C., the hot drawing single-mode deformation is 10%-20%, and the hot drawing rate is 1-3 m / min.

5. The method for preparing rare earth magnesium alloy wire for arc additive manufacturing according to claim 1, characterized in that: In the step 2, the spacing between the resistance butt welding fixtures is 1 to 3 mm, and the end faces are ensured to be strictly aligned, the preheating current is 50 to 80 A, the time is 0.05 to 0.1 s, and the top forging pressure is 0.02 to 0.06 MPa, the welding current is 100 to 200 A, the time is 0.3 to 0.6 s, and the top forging pressure is 0.1 to 0.3 MPa, the slow cooling current is 10 to 40 A, the time is 0.1 to 0.2 s, and the top forging pressure is 0 MPa.

6. The method for preparing rare earth magnesium alloy wire for arc additive manufacturing according to claim 1, characterized in that: In the step 3, the diameter of the reel used for peeling is Φ400mm; wherein, the first and second peeling passes only use a peeling die, the diameter reduction of a single die is 0.1-0.2mm, the peeling rate is 10-20m / min, and a magnesium alloy wire with a diameter of Φ1.25mm is obtained; the last peeling pass uses a combination die of a peeling die and a calendering die, and the corresponding peeling die diameter reduction is 0.03mm, the calendering die diameter reduction is 0.02mm, the peeling rate is 10m / min, and a magnesium alloy wire with a diameter of Φ1.25mm is obtained. Magnesium alloy wire.

Citation Information

Patent Citations

  • Magnesium alloy as well as preparation method and application thereof

    CN107099713A

  • Preparation method of rare earth magnesium alloy wire suitable for electric arc additive manufacturing

    CN114798799A

  • Device and method for preparing magnesium alloy wire for electric arc additive material through pulse current auxiliary roller die hot drawing

    CN116511274A

  • Magnesium alloy wire drawing method

    CN1554495A

  • Production method for magnesium alloy wire material

    JP2004017114A

Cited By

  • Forming process of special-shaped braided wire for heat pipe

    CN120232296A

  • Special-shaped braided wire forming process for heat pipe

    CN120232296B

  • High-performance low-cost magnesium alloy wire as well as preparation method and application thereof

    CN120905572A

  • High-toughness magnesium alloy wire material based on electric pulse annealing treatment and preparation method of high-toughness magnesium alloy wire material

    CN121592974A