A deep groove stress release bimetallic composite roller sleeve and its preparation method and application

By setting stress relief grooves on the outer roller sleeve of the bimetal composite roller sleeve and filling it with surfacing filler, combined with the design of the medium carbon steel inner roller sleeve, the problem of cracks in the roller sleeve during the heat treatment process is solved, and the roller sleeve is improved. The wear resistance and toughness extend the service life and reduce economic losses.

CN115945259BActive Publication Date: 2024-10-29NORTHEASTERN UNIV CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310059561.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-10-29
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

Bimetallic composite roller sleeves are prone to cracks during heat treatment, resulting in shortened service life and economic losses, and the wear-resistant layer is not tough enough to cope with strong wear conditions.

Method used

The deep groove stress relief bimetal composite roller sleeve design is adopted. The stress relief groove is set on the outer roller sleeve and filled with surfacing filler, and studs are embedded on the surface of the filler to release the phase change stress and thermal stress during the heat treatment process. , while using medium carbon steel as the inner roller sleeve to enhance the toughness of the roller sleeve.

Benefits of technology

It effectively prevents cracks in the roller sleeve during heat treatment and use, improves the wear resistance and toughness of the roller sleeve, extends the service life, and reduces production cycle delays and economic losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115945259B_ABST
    Figure CN115945259B_ABST
Patent Text Reader

Abstract

A deep groove stress release bimetallic composite roller sleeve and its preparation method and application belong to the field of bimetallic composite roller sleeves. The provided deep groove stress release bimetallic composite roller sleeve comprises an inner roller sleeve and an outer roller sleeve, wherein the outer roller sleeve is arranged on the outer periphery of the inner roller sleeve, and a plurality of stress release grooves are evenly distributed on the outer peripheral surface of the outer roller sleeve; the stress release grooves are filled with surfacing fillers, and studs are driven into the surface of the surfacing fillers to increase their wear resistance. The preparation is as follows: centrifugal casting of the outer roller sleeve and the inner roller sleeve, followed by annealing heat treatment, deep groove processing and filling with surfacing fillers, followed by quenching and tempering heat treatment, and studs are embedded in the surfacing of the roller sleeve. The deep groove stress release bimetallic composite roller sleeve has both good wear resistance and toughness. The set stress release groove can effectively release the phase change stress and thermal stress generated by martensitic phase transformation and the like during the heat treatment process, thereby reducing the risk of cracking of the deep groove stress release bimetallic roller sleeve during use, and is particularly suitable for high-pressure roller mills or roller presses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a deep groove stress release bimetallic composite roller sleeve and a preparation method and application thereof, belonging to the technical field of bimetallic composite roller sleeves, and more specifically to a deep groove stress release bimetallic composite roller sleeve and a preparation method thereof and application thereof in a high pressure roller mill / roller press. Background Art

[0002] High-pressure roller mill / roller press has the advantages of high efficiency and energy saving, and has been widely used in the fields of cement, ore and environmental protection at home and abroad. Wear-resistant roller sleeves are the main bearers of stress and wear during the use of high-pressure roller mill / roller press. At present, the types of roller sleeves mainly include tungsten carbide column nail embedded roller sleeves, wear-resistant material surfacing roller sleeves, bimetallic composite roller sleeves, etc. Column nail embedded roller sleeves have a long service life, but the price is relatively expensive; wear-resistant material surfacing roller sleeves are prone to cracks and other defects under strong wear conditions, causing the surfacing wear-resistant layer to fall off, seriously reducing its service life and extending the production cycle. Therefore, under strong wear conditions, the roller sleeve needs to have both good wear resistance and good toughness. In view of this, bimetallic composite roller sleeves came into being, which improved the comprehensive performance of the roller sleeve to a certain extent.

[0003] The outer layer of the bimetallic composite roller sleeve is usually made of a relatively wear-resistant material, and the inner layer is made of medium-carbon alloy steel. After the roller sleeve is formed, it needs to be subjected to final heat treatment before it can be used. Since the outer layer is a highly wear-resistant alloy, it usually has higher hardness, better wear resistance and lower toughness. Although heat treatment will improve the wear resistance of the grinding roller, it will reduce its toughness to a certain extent, making it easy to crack during use, shortening its service life and even causing danger. The wear-resistant layer on its outer surface also has the risk of cracking during the heat treatment process, and the cracks will extend to the inner layer, which will cause economic losses and is not conducive to energy conservation and environmental protection. If the hardness of the outer roller sleeve reaches 60-65HRC, it will have good wear resistance, but it is easy to crack; if the hardness of the outer roller sleeve is between 55-60HRC, the risk of roller sleeve cracking can be effectively reduced, but the wear resistance decreases, which seriously reduces the service life of the bimetallic composite roller sleeve. Therefore, in this field, how to ensure the high hardness of the outer roller sleeve while effectively preventing the wear-resistant layer of the bimetallic composite roller sleeve from cracking during heat treatment and subsequent use is an urgent problem to be solved in this field. Summary of the invention

[0004] In view of the problems of the prior art, in order to prevent the wear-resistant layer of the bimetallic composite roller sleeve from cracking during the heat treatment process, the present invention solves the above problems by releasing the surface tissue stress and thermal stress on the basis of the existing bimetallic composite roller sleeve. Therefore, a deep groove stress release bimetallic composite roller sleeve and its preparation method and application are proposed, especially in the application of high-pressure roller mill / roller press. The deep groove stress release bimetallic composite roller sleeve is made of medium carbon steel with good toughness as the inner roller sleeve and high wear-resistant material as the outer roller sleeve, and a stress release groove is provided on the outer roller sleeve, and the stress release groove is filled with a surfacing filler, and studs are driven into the surface of the surfacing filler to increase its wear resistance. The deep groove stress release bimetallic composite roller sleeve produced by the preparation method has both good wear resistance and good toughness. On the one hand, the composition of the roller sleeve can be precisely controlled, and the outer roller sleeve adopts a high wear-resistant material to play a wear-resistant role. On the other hand, the inner roller sleeve is a toughness layer, which plays a toughening role on the deep groove stress release bimetallic composite roller sleeve as a whole, effectively reducing the risk of cracking of the deep groove stress release bimetallic composite roller sleeve during use. At the same time, the outer roller sleeve is provided with a stress relief groove, which can reduce the risk of cracking of the roller sleeve during use and heat treatment. The stress relief groove of the present invention is a deep groove equally separated along the direction of the cylindrical generatrix and runs through the entire outer roller sleeve. The stress relief groove can effectively release the phase change stress and thermal stress generated by martensitic phase transformation and the like during heat treatment.

[0005] The present invention discloses a deep groove stress release bimetallic composite roller sleeve, comprising an inner roller sleeve and an outer roller sleeve, wherein the outer roller sleeve is arranged on the outer periphery of the inner roller sleeve, and a plurality of stress release grooves are evenly distributed on the outer periphery of the outer roller sleeve; the stress release grooves are filled with a cladding filler, studs are embedded on the surface of the cladding filler, and the studs extend into the inner roller sleeve to increase the wear resistance of the deep groove stress release bimetallic composite roller sleeve.

[0006] Furthermore, the inner roller sleeve material is ordinary medium carbon steel or medium carbon alloy steel.

[0007] The outer roller sleeve adopts a highly wear-resistant material having the following chemical components and the mass percentage of each component: C: 0.1-4.0%, Si: 0.1-1.5%, Mn: 0-15%, Cr: 5-30%, Mo: 0-20%, B: 0-5%, W: 0-15%, V: 0-8%, Ni: 0-3%, Nb: 0-6%, Ti: 0-5%, and the balance is Fe and unavoidable impurities;

[0008] The thickness of the outer roller sleeve is 30-60mm.

[0009] Furthermore, each stress relief groove coincides with a generatrix of the outer roller sleeve.

[0010] The number of the stress release grooves is preferably 4-12 and are evenly distributed along the generatrix direction.

[0011] The stress release groove is opened on the outer roller sleeve and is a through groove, and its depth is the same as or greater than the thickness of the outer roller sleeve. The stress release groove is an arc-shaped trapezoidal structure, and the angle of the side wall of the stress release groove is 5 to 30 degrees.

[0012] The stud material is TiC, WC or other highly wear-resistant materials, and the size is The distance between the studs of the cladding filler and the inner roller sleeve at each stress relief groove is 10-20mm. According to the application of the roller mill, the stud material should be reasonably selected so that it can wear synchronously with the roller sleeve surface.

[0013] The cladding filler is preferably one of martensitic steel and austenitic steel;

[0014] The column nails are preferably arranged in 1 to 2 rows.

[0015] The deep groove stress release bimetal composite roller sleeve of the present invention has an outer roller sleeve surface Rockwell hardness of 60-65HRC, an inner roller sleeve hardness of 30-40HRC, a shear strength between the inner roller sleeve and the outer roller sleeve of 500-580Mpa, and an outer roller sleeve impact toughness of 3-12J / cm 2 .

[0016] A method for preparing a deep groove stress release bimetallic composite roller sleeve of the present invention specifically comprises the following steps:

[0017] Step 1: Preparation of the outer roller cover

[0018] The alloy of the outer roller sleeve is selected, and the chemical composition and mass percentage of each component contained in the outer roller sleeve are: C: 0.1-4.0%, Si: 0.1-1.5%, Mn: 0-15%, Cr: 5-30%, Mo: 0-20%, B: 0-5%, W: 0-15%, V: 0-8%, Ni: 0-3%, Nb: 0-6%, Ti: 0-5%, and the balance is Fe and inevitable impurities; conventional centrifugal casting process is used for casting, and the thickness is 30-60mm, so as to obtain the outer roller sleeve of the bimetallic composite roller sleeve;

[0019] Step 2: Preparation of the inner roller cover

[0020] Ordinary medium carbon steel or medium carbon alloy steel is selected and cast on the inner side of the outer roller sleeve by centrifugal casting process, wherein the inner side of the outer roller sleeve is in a semi-solid zone to obtain a bimetallic composite roller sleeve;

[0021] Step 3: Heat treatment of bimetallic composite roller sleeve:

[0022] The bimetallic composite roller sleeve is heat treated as a whole to obtain a heat-treated bimetallic composite roller sleeve; the heat treatment process of the bimetallic composite roller sleeve is as follows:

[0023] annealing:

[0024] Annealing temperature: 400~700℃

[0025] Heating rate: 7~10℃ / min

[0026] Insulation time: 5-20h

[0027] Cooling method: furnace cooling;

[0028] Step 4: Deep groove processing

[0029] (1) A deep groove is made on the outer roller sleeve of the heat-treated bimetallic composite roller sleeve, the depth of which is 1-1.5 times the thickness of the outer roller sleeve, and the corners are rounded at the opening to obtain a bimetallic composite roller sleeve with a groove;

[0030] (2) Treat the inner surface of the groove on the outer roller sleeve of the bimetallic composite roller sleeve to make it clean and smooth;

[0031] (3) Fill each deep groove with cladding filler, and the hardness of the cladding filler is 45-50HRC;

[0032] (4) performing surface treatment on the surfacing portion to make it flush with the outer roller sleeve, thereby obtaining a bimetallic composite roller sleeve with a stress relief groove;

[0033] Step 5: Heat Treatment of Bimetallic Composite Roller Sleeve with Stress Relief Grooves

[0034] The heat treatment process of the bimetallic composite roller sleeve with stress relief groove is:

[0035] (1) Quenching: The bimetallic composite roller sleeve with stress release groove is quenched to obtain an air-cooled bimetallic composite roller sleeve with stress release groove. The specific quenching process is as follows:

[0036] Quenching temperature: 1000~1080℃

[0037] Heating rate: 7~10℃ / min

[0038] Insulation time: 5 to 15 hours

[0039] Cooling method: air cooling

[0040] (2) Tempering: The bimetallic composite roller sleeve with stress release groove after air cooling is tempered to obtain a heat-treated roller sleeve. The specific process of tempering is as follows:

[0041] Tempering temperature: 300~600℃

[0042] Heating rate: 7~10℃ / min

[0043] Insulation time: 1 to 15 hours

[0044] Cooling method: Furnace cooling

[0045] Step 6: Embedding studs: Embed studs at the roller sleeve surfacing after heat treatment in step 5 to obtain a deep groove stress relief bimetallic composite roller sleeve.

[0046] In the step 2, the ordinary medium carbon steel or medium carbon alloy steel is one of 35 steel, 40 steel, 45 steel or 50 steel;

[0047] In step 4(2), the surface is treated, including mechanical processing to remove oxide scale, and cleaning with an organic solvent such as alcohol to obtain a clean surface.

[0048] Furthermore, in step 4 (4), 1 to 2 rows of column nails are driven along the circumference of the outer roller sleeve.

[0049] The deep groove stress release bimetallic composite roller sleeve prepared by the preparation method realizes metallurgical bonding between the inner roller sleeve and the outer roller sleeve, between the inner roller sleeve and the cladding filler in the stress release groove, and between the outer roller sleeve and the cladding filler in the stress release groove.

[0050] The deep groove stress release bimetal composite roller sleeve of the present invention can effectively prevent cracks from being generated during heat treatment and use, and is particularly suitable for high-pressure roller mills or roller presses.

[0051] Compared with the prior art, the deep groove stress release bimetallic composite roller sleeve of the present invention and its preparation method and application have the following characteristics:

[0052] (1) The inner roller sleeve of the deep groove stress release bimetallic composite roller sleeve of the present invention is made of medium carbon steel with relatively excellent impact toughness, and the outer roller sleeve is made of wear-resistant alloy. The organic combination of the two and the matching stress release groove greatly improve the toughness and wear resistance of the bimetallic composite roller sleeve.

[0053] (2) The deep groove stress release bimetallic composite roller sleeve of the present invention has an outer roller sleeve provided with a stress release groove, which greatly reduces the risk of cracking of the roller sleeve during heat treatment and use. The stress release groove is set at an angle to facilitate the processing of the groove and the filling of fillers; the addition of surfacing fillers at the stress release groove can, on the one hand, prevent the grooved roller sleeve from cracking during use, and on the other hand, it is also a carrier for the studs, further increasing the wear resistance of the roller sleeve. It avoids risks, saves energy and protects the environment, improves production safety, and effectively avoids the extension of the production cycle due to cracking of the roller sleeve;

[0054] (3) The inner roller sleeve of the deep groove stress release bimetallic composite roller sleeve of the present invention is made of low-cost medium carbon steel, which greatly reduces its production cost and is suitable for large-scale batch production;

[0055] (4) The outer roller sleeve of the deep groove stress release bimetallic composite roller sleeve of the present invention is compositely added with multiple alloy elements, the composition is controllable, the production stability can be achieved, the wear resistance of the alloy is greatly improved, the service life is extended, and the construction delay caused by replacing the roller sleeve is saved.

[0056] (5) The deep groove stress release bimetallic composite roller sleeve for high pressure roller mill / roller press prepared by the present invention is well combined with the inner roller sleeve and the outer roller sleeve of the bimetallic composite roller sleeve after centrifugal casting and subsequent heat treatment, without obvious defects such as holes and cracks;

[0057] (6) A deep groove stress release bimetallic composite roller sleeve of the present invention has a rounded corner at the opening of the stress release groove, thereby avoiding the risk of the roller sleeve getting stuck during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a schematic structural diagram of the deep groove stress release bimetallic composite roller sleeve of the present invention;

[0059] Among them, 1 is the outer roller sleeve, 2 is the inner roller sleeve, 3 is the stress relief groove, 4 is the column nail, and 5 is the surfacing filler;

[0060] Figure 2 It is a schematic front view of the stress release groove of the deep groove stress release bimetallic composite roller sleeve of the present invention;

[0061] In the figure, 1 is an outer roller sleeve, 5 is a surfacing material, and 4 is a column nail;

[0062] Figure 3 It is a top view of the stress release groove of the bimetallic composite roller sleeve with deep groove stress release in the present invention;

[0063] Figure 4 Schematic diagram of the interface between the inner roller sleeve and the outer roller sleeve in the deep groove stress release bimetallic composite roller sleeve of Example 4 of the present invention, wherein 1 is the outer roller sleeve, 2 is the inner roller sleeve, and 6 is the interface bonding layer between the inner and outer roller sleeves;

[0064] Figure 5 The hardness distribution at the interface between the inner roller sleeve and the outer roller sleeve in the deep groove stress release bimetallic composite roller sleeve of Example 3 of the present invention;

[0065] Figure 6 The present invention is a process flow chart of the deep groove stress release bimetallic composite roller sleeve. DETAILED DESCRIPTION

[0066] The present invention is further described in detail below in conjunction with the embodiments and drawings.

[0067] Example 1

[0068] A method for preparing a bimetallic composite roller sleeve of the present invention, the process flow chart of which is shown in Figure 6 , specifically including the following steps:

[0069] Step 1: Preparation of the outer roller cover

[0070] The chemical composition and mass percentage of each component of the alloy of the outer roller sleeve are selected as follows: C: 0.1%, Si: 1.5%, Mn: 2%, Cr: 30%, Mo: 0%, B: 3%, W: 7%, V: 8%, Ni: 2%, Nb: 0%, Ti: 5%, and the balance is Fe and inevitable impurities; the outer roller sleeve of the bimetallic composite roller sleeve is cast by a conventional centrifugal casting process, and the thickness is 30 mm, so as to obtain the outer roller sleeve of the bimetallic composite roller sleeve;

[0071] Step 2: Preparation of the inner roller cover

[0072] No. 40 steel is selected and cast immediately on the inner side of the outer roller sleeve by centrifugal casting process (the inner side of the outer roller sleeve is in a semi-solid zone) to obtain a bimetallic composite roller sleeve;

[0073] Step 3, heat treatment of bimetallic composite roller sleeve:

[0074] The bimetallic composite roller sleeve in step 2 is heat treated as a whole to obtain a heat-treated bimetallic composite roller sleeve; the heat treatment process of the bimetallic composite roller sleeve is:

[0075] annealing:

[0076] Annealing temperature: 400℃

[0077] Heating rate: 7℃ / min

[0078] Insulation time: 20h

[0079] Cooling method: furnace cooling

[0080] Step 4: Deep groove processing

[0081] (1) The outer roller sleeve of the heat-treated bimetallic composite roller sleeve obtained in step 3 is provided with a deep groove as a stress release groove, the depth of which is 1.5 times the thickness of the outer roller sleeve, and the opening is rounded; the rounded corner R is 1-6 mm, and the side wall angle of the stress release groove is 30°; the number of the stress release grooves is 4, which are evenly distributed in the generatrix direction around the outer roller sleeve; and penetrate the outer roller sleeve;

[0082] (2) machining the inner surface of the groove on the outer roller sleeve of the bimetallic composite roller sleeve obtained in (1) to remove the oxide scale and washing it with an organic solvent such as alcohol to make it clean and smooth;

[0083] (3) Fill each deep groove with cladding filler;

[0084] (4) Drive a row of studs with a size of The stud spacing between the cladding filler and the inner roller sleeve at each stress relief groove is 20mm;

[0085] (5) performing surface treatment on the surfacing filler to make it flush with the outer roller sleeve, thereby obtaining a bimetallic composite roller sleeve with a stress relief groove;

[0086] Step 5: Heat Treatment of Bimetallic Composite Roller Sleeve with Stress Relief Grooves

[0087] The heat treatment process of the bimetallic composite roller sleeve with stress relief groove is:

[0088] (1) Quenching: The bimetallic composite roller sleeve treated in step 4 is quenched as a whole to obtain a bimetallic composite roller sleeve with a stress release groove after air cooling. The specific quenching process is as follows:

[0089] Quenching temperature: 1080℃

[0090] Heating rate: 10℃ / min

[0091] Insulation time: 10h

[0092] Cooling method: air cooling

[0093] (2) Tempering: The bimetallic composite roller sleeve after air cooling is tempered as a whole to obtain a heat-treated roller sleeve. The specific process of tempering is as follows:

[0094] Tempering temperature: 300℃

[0095] Heating rate: 10℃ / min

[0096] Insulation time: 1h

[0097] Cooling method: Furnace cooling

[0098] Step 6: Inlaying studs: Inlay studs at the roller sleeve surfacing after heat treatment in step 5 to obtain a deep groove stress release bimetallic composite roller sleeve. The schematic diagram of its structure is shown in Figure 1 , including an inner roller sleeve 2 and an outer roller sleeve 1, the outer roller sleeve 1 is sleeved on the outer periphery of the inner roller sleeve 2, and a plurality of stress release grooves 3 are evenly distributed on the outer periphery of the outer roller sleeve 1; the stress release grooves 3 are filled with cladding fillers 5, and studs 4 are used to connect the cladding fillers 5 and the inner roller sleeve 2.

[0099] The deep groove stress release bimetal composite roller sleeve of the present invention has a surface Rockwell hardness of 60HRC for the outer roller sleeve, a shear strength of 550Mpa between the inner roller sleeve and the outer roller sleeve, and an impact toughness of 10J / cm 2 The composite roller sleeve is dense and has no obvious cracks or other defects. The main schematic diagram of the stress release groove of the deep groove stress release bimetallic composite roller sleeve in this embodiment is shown in Figure 2 , wherein 1 is an outer roller sleeve, 5 is a cladding filler, and 4 is a column nail; a top view of the stress release groove of the deep groove stress release bimetallic composite roller sleeve of the present invention is shown in Figure 3 .

[0100] Example 2

[0101] A method for preparing a deep groove stress release bimetallic composite roller sleeve of the present invention specifically comprises the following steps:

[0102] Step 1: Preparation of the outer roller cover

[0103] The chemical composition and mass percentage of each component of the alloy of the outer roller sleeve are selected as follows: C: 4%, Si: 0.1%, Mn: 15%, Cr: 5%, Mo: 3%, B: 0%, W: 10%, V: 0%, Ni: 3%, Nb: 6%, Ti: 0%, and the balance is Fe and inevitable impurities; the outer roller sleeve of the bimetallic composite roller sleeve is cast by a conventional centrifugal casting process, and the thickness is 30 mm, so as to obtain the outer roller sleeve of the bimetallic composite roller sleeve;

[0104] Step 2: Preparation of the inner roller cover

[0105] Select No. 35 steel and use centrifugal casting process to cast it immediately on the inner side of the outer roller sleeve (the inner side of the outer roller sleeve is in a semi-solid zone) to obtain a bimetallic composite roller sleeve;

[0106] Step 3, heat treatment of bimetallic composite roller sleeve:

[0107] The bimetallic composite roller sleeve in step 2 is heat treated as a whole to obtain a heat-treated bimetallic composite roller sleeve; the heat treatment process of the bimetallic composite roller sleeve is:

[0108] annealing:

[0109] Annealing temperature: 700℃

[0110] Heating rate: 10℃ / min

[0111] Insulation time: 5h

[0112] Cooling method: furnace cooling

[0113] Step 4: Deep groove processing

[0114] (1) The outer roller sleeve of the heat-treated bimetallic composite roller sleeve obtained in step 3 is provided with deep grooves as stress release grooves, the depth of which is 1 times the thickness of the outer roller sleeve, and the corners are rounded at the opening to obtain a bimetallic composite roller sleeve with grooves; the corner radius R is 3 mm; the number of stress release grooves is 4, which are evenly distributed in the generatrix direction around the outer roller sleeve; and penetrate the outer roller sleeve;

[0115] (2) machining the inner surface of the groove on the outer roller sleeve of the bimetallic composite roller sleeve obtained in (1) to remove the oxide scale and washing it with an organic solvent such as alcohol to make it clean and smooth;

[0116] (3) Fill each deep groove with cladding filler;

[0117] (4) Drive a row of studs with a size of The stud spacing between the cladding filler and the inner roller sleeve at each stress relief groove is 20mm;

[0118] (5) performing surface treatment on the surfacing filler to make it flush with the outer roller sleeve, thereby obtaining a bimetallic composite roller sleeve with a stress relief groove;

[0119] Step 5: Heat Treatment of Bimetallic Composite Roller Sleeve with Stress Relief Grooves

[0120] The heat treatment process of the bimetallic composite roller sleeve with stress relief groove is:

[0121] (1) Quenching: The bimetallic composite roller sleeve treated in step 4 is quenched as a whole to obtain a bimetallic composite roller sleeve with a stress release groove after air cooling. The specific quenching process is as follows:

[0122] Quenching temperature: 1000℃

[0123] Heating rate: 7℃ / min

[0124] Insulation time: 15h

[0125] Cooling method: air cooling

[0126] (2) Tempering: The bimetallic composite roller sleeve after air cooling is tempered as a whole to obtain a heat-treated roller sleeve. The specific process of tempering is as follows:

[0127] Tempering temperature: 600℃

[0128] Heating rate: 7℃ / min

[0129] Insulation time: 15h

[0130] Cooling method: Furnace cooling

[0131] Step 6: Embedding studs: Embed studs at the roller sleeve surfacing after heat treatment in step 5 to obtain a deep groove stress relief bimetallic composite roller sleeve.

[0132] The deep groove stress release bimetal composite roller sleeve of the present invention can be used in a high pressure roller mill / roller press, the outer roller sleeve surface Rockwell hardness is 60HRC, the shear strength between the inner and outer roller sleeves is 500Mpa, and the impact toughness of the outer roller sleeve is 12J / cm 2 The composite roller sleeve is dense and has no obvious cracks or other defects.

[0133] Example 3

[0134] A method for preparing a deep groove stress release bimetallic composite roller sleeve of the present invention specifically comprises the following steps:

[0135] Step 1: Preparation of the outer roller cover

[0136] The chemical composition and mass percentage of each component of the alloy of the outer roller sleeve are selected as C: 0.1%, Si: 0.5%, Mn: 0%, Cr: 5%, Mo: 2%, B: 5%, W: 15%, and the balance is Fe and inevitable impurities; the outer roller sleeve of the bimetallic composite roller sleeve is cast by a conventional centrifugal casting process, and the thickness is 60 mm;

[0137] Step 2: Preparation of the inner roller cover

[0138] Select No. 60 steel and use centrifugal casting process to cast it immediately on the inner side of the outer roller sleeve (the inner side of the outer roller sleeve is in a semi-solid zone) to obtain a bimetallic composite roller sleeve;

[0139] Step 3, heat treatment of bimetallic composite roller sleeve:

[0140] The bimetallic composite roller sleeve in step 2 is heat treated as a whole to obtain a heat-treated bimetallic composite roller sleeve; the heat treatment process of the bimetallic composite roller sleeve is:

[0141] annealing:

[0142] Annealing temperature: 500℃

[0143] Heating rate: 10℃ / min

[0144] Insulation time: 10h

[0145] Cooling method: furnace cooling

[0146] Step 4: Deep groove processing

[0147] (1) The outer roller sleeve of the heat-treated bimetallic composite roller sleeve obtained in step 3 is provided with deep grooves as stress release grooves, the depth of which is 1 times the thickness of the outer roller sleeve, and the corners are rounded at the opening; the rounded corner R is 6 mm; the number of stress release grooves is 4, which are evenly distributed in the generatrix direction around the outer roller sleeve; and penetrate the outer roller sleeve;

[0148] (2) machining the inner surface of the groove on the outer roller sleeve of the bimetallic composite roller sleeve obtained in (1) to remove the oxide scale and washing it with an organic solvent such as alcohol to make it clean and smooth;

[0149] (3) Fill each deep groove with cladding filler;

[0150] (4) Drive two rows of studs along the axial direction of the outer roller sleeve at the cladding filler. The stud spacing between the cladding filler and the inner roller sleeve at each stress relief groove is 10mm;

[0151] (5) performing surface treatment on the surfacing filler to make it flush with the outer roller sleeve, thereby obtaining a bimetallic composite roller sleeve with a stress relief groove;

[0152] Step 5: Heat Treatment of Bimetallic Composite Roller Sleeve with Stress Relief Grooves

[0153] The heat treatment process of the bimetallic composite roller sleeve with stress relief groove is:

[0154] (1) Quenching: The bimetallic composite roller sleeve treated in step 4 is quenched as a whole to obtain a bimetallic composite roller sleeve with a stress release groove after air cooling. The specific quenching process is as follows:

[0155] Quenching temperature: 1040℃

[0156] Heating rate: 8℃ / min

[0157] Insulation time: 6h

[0158] Cooling method: air cooling

[0159] (2) Tempering: The bimetallic composite roller sleeve after air cooling is tempered as a whole to obtain a heat-treated roller sleeve. The specific process of tempering is as follows:

[0160] Tempering temperature: 550℃

[0161] Heating rate: 8℃ / min

[0162] Insulation time: 3h

[0163] Cooling method: Furnace cooling

[0164] Step 6: Embedding studs: Embed studs at the roller sleeve surfacing after heat treatment in step 5 to obtain a deep groove stress relief bimetallic composite roller sleeve.

[0165] The deep groove stress release bimetal composite roller sleeve of the present invention can be used in a high pressure roller mill / roller press, the outer roller sleeve surface Rockwell hardness is 68HRC, the shear strength between the inner and outer roller sleeves is 520Mpa, and the impact toughness of the outer roller sleeve is 3J / cm 2 The fiber hardness distribution at the interface of the inner and outer roller sleeves is as follows: Figure 5 As shown in the figure, the composite roller sleeve is dense and has no obvious cracks or other defects.

[0166] Example 4

[0167] Same as Example 3, except that the chemical composition and mass percentage of each component contained in the outer roller sleeve alloy are: C: 2%, Si: 1%, Mn: 1%, Cr: 10%, Mo: 20%, B: 1.5%, W: 0%, and the balance is Fe and unavoidable impurities;

[0168] (1) Quenching: The bimetallic composite roller sleeve treated in step 4 is quenched as a whole to obtain a bimetallic composite roller sleeve with a stress release groove after air cooling. The specific quenching process is as follows:

[0169] Quenching temperature: 1040℃

[0170] Heating rate: 9℃ / min

[0171] Insulation time: 5h

[0172] Cooling method: air cooling

[0173] (2) Tempering: The bimetallic composite roller sleeve after air cooling is tempered as a whole to obtain a heat-treated roller sleeve. The specific process of tempering is as follows:

[0174] Tempering temperature: 500℃

[0175] Heating rate: 9℃ / min

[0176] Insulation time: 3h

[0177] Cooling method: Furnace cooling

[0178] The bimetal composite roller sleeve for high pressure roller mill / roller press of the present invention has an outer roller sleeve surface Rockwell hardness of 65HRC, a shear strength between the inner and outer roller sleeves of 580Mpa, and an outer roller sleeve impact toughness of 8J / cm 2 The composite roller sleeve is dense and has no obvious cracks or other defects.

[0179] And the schematic diagram of the interface between the inner roller sleeve and the outer roller sleeve in the deep groove stress release bimetallic composite roller sleeve is shown in Figure 4It can be seen that an interface bonding layer 6 is formed between the outer roller sleeve 1 and the inner roller sleeve 2, and the bonding thickness of the interface bonding layer 6 is 30-60 μm. Moreover, after testing, metallurgical bonding is achieved between the inner roller sleeve and the cladding filler in the stress release groove, and between the outer roller sleeve and the cladding filler in the stress release groove.

[0180] Example 5

[0181] Same as Example 1, except that 45 steel and conventional process are selected for casting; the quenching temperature is 1040°C, the deep groove stress release bimetallic composite roller sleeve of the present invention has a surface Rockwell hardness of 65HRC on the outer roller sleeve, a shear strength between the inner and outer roller sleeves of 554Mpa, and an impact toughness of 11J / cm 2 The composite roller sleeve is dense and has no obvious cracks or other defects.

[0182] Comparative Example 1

[0183] A vertical stress relief groove, that is, a stress relief groove with a side wall angle of 90°, is difficult to process and is not conducive to filling with fillers.

[0184] Comparative Example 2

[0185] A method for preparing a bimetallic composite roller sleeve is the same as that of Example 1, except that the bimetallic composite roller sleeve is not subjected to heat treatment in step 3, and is directly subjected to the whole-body treatment in step 5, thereby reducing the toughness of the roller sleeve.

Claims

1. A deep groove stress release bimetallic composite roller sleeve, characterized in that: It comprises an inner roller sleeve and an outer roller sleeve, wherein the outer roller sleeve is arranged on the outer periphery of the inner roller sleeve, and a plurality of stress release grooves are evenly distributed on the outer periphery of the outer roller sleeve; the stress release grooves are filled with cladding fillers, and studs are driven into the surface of the cladding fillers to increase their wear resistance; Wherein, the inner roller sleeve material is ordinary medium carbon steel or medium carbon alloy steel; The outer roller sleeve adopts a highly wear-resistant material, and the chemical composition and mass percentage of each component are: C: 0.1-4.0%, Si: 0.1-1.5%, Mn: 0-15%, Cr: 5-30%, Mo: 0-20%, B: 0-5%, W: 0-15%, V: 0-8%, Ni: 0-3%, Nb: 0-6%, Ti: 0-5%, and the balance is Fe and unavoidable impurities; the thickness of the outer roller sleeve is 30-60mm; The stress release groove is opened on the outer roller sleeve and is a through groove. Each stress release groove coincides with the generatrix of the outer roller sleeve. The number of stress release grooves is 4-12 and is evenly distributed along the generatrix direction. The depth is the same as or greater than the thickness of the outer roller sleeve. The stress release groove is an arc-shaped trapezoidal structure, and the angle of the side wall of the stress release groove is 5-30°.

2. The deep groove stress release bimetallic composite roller sleeve according to claim 1 is characterized in that: The surfacing filler is one of martensitic steel and austenitic steel.

3. The deep groove stress release bimetallic composite roller sleeve according to claim 1, characterized in that: The stud material is TiC, WC or one of other highly wear-resistant materials, with a size of φ10-20mm. The stud spacing between the cladding filler at each stress release groove and the inner roller sleeve is 10-20mm. The corresponding stud material is selected according to the application of the roller mill so that it wears synchronously with the roller sleeve surface.

4. The deep groove stress release bimetallic composite roller sleeve according to any one of claims 1 to 3, characterized in that: The Rockwell hardness of the outer roller cover is 60-65HRC, and the hardness of the inner roller cover is 30-40HRC; the shear strength between the inner roller cover and the outer roller cover is 500-580Mpa, and the impact toughness of the outer roller cover is 3-12J / cm 2 Metallurgical bonding is achieved between the inner roller sleeve and the outer roller sleeve, between the inner roller sleeve and the cladding filler in the stress release groove, and between the outer roller sleeve and the cladding filler in the stress release groove.

5. The method for preparing the deep groove stress release bimetallic composite roller sleeve according to any one of claims 1 to 3, characterized in that: The specific steps include: Step 1: Preparation of the outer roller cover The alloy of the outer roller sleeve is selected, and the chemical composition and mass percentage of each component contained in the outer roller sleeve are: C: 0.1-4.0%, Si: 0.1-1.5%, Mn: 0-15%, Cr: 5-30%, Mo: 0-20%, B: 0-5%, W: 0-15%, V: 0-8%, Ni: 0-3%, Nb: 0-6%, Ti: 0-5%, and the balance is Fe and inevitable impurities; conventional centrifugal casting process is used for casting, and the thickness is 30-60mm, so as to obtain the outer roller sleeve of the bimetallic composite roller sleeve; Step 2: Preparation of the inner roller cover Ordinary medium carbon steel or medium carbon alloy steel is selected and cast on the inner side of the outer roller sleeve by centrifugal casting process, wherein the inner side of the outer roller sleeve is in a semi-solid zone to obtain a bimetallic composite roller sleeve; Step 3: Heat treatment of bimetallic composite roller sleeve: The bimetallic composite roller sleeve is heat treated as a whole to obtain a heat-treated bimetallic composite roller sleeve; the heat treatment process of the bimetallic composite roller sleeve is as follows: Annealing: Annealing temperature: 400-700℃, heating rate: 7-10℃ / min, holding time: 5-20h, cooling method: furnace cooling; Step 4: Deep groove processing (1) A deep groove is made on the outer roller sleeve of the heat-treated bimetallic composite roller sleeve, the depth of which is 1-1.5 times the thickness of the outer roller sleeve, and the corners are rounded at the opening to obtain a bimetallic composite roller sleeve with a groove; (2) Treat the inner surface of the groove on the outer roller sleeve of the bimetallic composite roller sleeve to make it clean and smooth; (3) Fill each deep groove with cladding filler, and the hardness of the cladding filler is 45-50HRC; (4) Surface treatment is performed on the surfacing portion to make it flush with the outer roller sleeve, thereby obtaining a bimetallic composite roller sleeve with a stress relief groove; Step 5: Heat Treatment of Bimetallic Composite Roller Sleeve with Stress Relief Grooves The heat treatment process of the bimetallic composite roller sleeve with stress relief groove is: (1) Quenching: The bimetallic composite roller sleeve with stress release groove is quenched to obtain the bimetallic composite roller sleeve with stress release groove after air cooling. The specific quenching process is as follows: quenching temperature: 1000-1080°C, heating rate: 7-10°C / min, holding time: 5-15h, cooling method: air cooling; (2) Tempering: The bimetallic composite roller sleeve with stress release groove after air cooling is tempered to obtain a heat-treated roller sleeve. The specific tempering process is as follows: tempering temperature: 300-600°C, heating rate: 7-10°C / min, holding time: 1-15h, cooling method: furnace cooling; Step 6: Install the studs: In step 5, studs are embedded in the surfacing of the roller sleeve after heat treatment to obtain a deep groove stress release bimetallic composite roller sleeve.

6. Application of the deep groove stress release bimetallic composite roller sleeve according to any one of claims 1 to 3 in a high pressure roller mill or a roller press.

Citation Information

Patent Citations

  • Column nail roller surface repairing method of novel high-pressure roller mill

    CN104526248A

  • Motor stator shell and motor

    CN112653257A

  • Armor nail roller sleeve and preparation method thereof

    CN114950636A