Laser welding method of TRIP steel-aluminum alloy with titanium / nickel composite intermediate layer

By using a titanium/nickel composite intermediate layer in the welding of aluminum alloy and TRIP steel, a tough phase is formed, which inhibits the generation of brittle intermetallic compounds, solves the problem of brittleness of the welded joint, and significantly improves the mechanical properties and connectivity of the welded joint.

CN115945783BActive Publication Date: 2024-10-15JILIN UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211637253.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-10-15
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

During the welding of aluminum alloys and TRIP steels, due to differences in crystal structure and physical and chemical properties, brittle intermetallic compounds are excessively generated at the welded joints, resulting in poor brittleness of the materials at low temperatures and reduced strength at high temperatures, making it difficult to achieve efficient connections.

Method used

The TRIP steel-aluminum alloy laser welding method using a titanium/nickel composite intermediate layer is used to sandwich pure nickel and pure titanium metal sheets in the welding area to form ductile phases such as Ni-Al and Fe2Ti to suppress the generation of brittle Fe-Al metal compounds. , improve the mechanical properties of welded joints.

Benefits of technology

Significantly improves the tensile and shear performance of the welded joint, there is no spatter during the welding process, the weld is smooth, the grain structure is fine, the heat affected zone is narrow, the tensile and shear performance is increased by more than 35%, which is better than the welding method of pure nickel and pure titanium intermediate layer .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115945783B_ABST
    Figure CN115945783B_ABST
Patent Text Reader

Abstract

The present invention provides a TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer, comprising the following steps: grinding, cleaning and drying the surface of the overlapped portion of the aluminum alloy sheet to be welded and the TRIP800 steel sheet; horizontally overlapping the aluminum alloy sheet at the bottom and the TRIP800 steel sheet at the top, sandwiching a composite intermediate layer in the overlapped area, the composite intermediate layer consisting of a pure nickel metal sheet at the bottom and a pure titanium metal sheet at the top; adjusting the motion path of the laser welding equipment and the preset weld to the same straight line, setting welding parameters, and laser welding the overlapped area of ​​the aluminum alloy sheet and the TRIP800 steel sheet. The TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer can effectively suppress the excessive generation of brittle intermetallic compounds at the welded joint, optimize the mechanical properties of the welded joint, improve the connectivity of steel and aluminum dissimilar metals, and the welding process is also simpler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of laser welding of dissimilar materials, and in particular to a TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer added. Background Art

[0002] TRIP steel, or Transformation Induced Plasticity Steel, uses the transformation induced plasticity effect to induce martensite nucleation under plastic deformation in the retained austenite in the steel plate, introduces the mechanism of phase transformation strengthening and plastic growth, and improves the strength and toughness of the steel plate. Since the discovery of the TRIP effect, efforts have been made all over the world to develop and produce high-quality TRIP steel in order to put it into industrial production. TRIP steel developed in the 1960s added too many alloy elements, resulting in high manufacturing costs. In order to obtain more stable retained austenite, complex heat treatment processes were required. Limited by the conditions at the time, the TRIP steel produced could not be applied to large-sized workpieces and welded parts, thus greatly limiting the application of TRIP steel. In the 1980s, the TRIP effect was also discovered in low-alloy steel, and steel that could still produce the TRIP effect after continuous annealing was produced, making the application of TRIP steel in the automotive field possible.

[0003] TRIP steel has a multiphase structure, which is a mixture of soft phase ferrite, hard phase bainite and metastable residual austenite, so that the residual austenite can be gradually transformed into martensite during the deformation process. The organizational properties of TRIP steel give it excellent mechanical properties, high strength and high plasticity. Ferrite is a soft phase structure, which can deform bainite during the stretching process, and bainite can improve the strength of TRIP steel; austenite is transformed into martensite when stretched at room temperature, and martensite produces stress relaxation during the phase transformation process, which increases plasticity. The martensite produced by the phase transformation can strengthen TRIP steel and increase the strength of TRIP steel. TRIP800 is another masterpiece of Anshan Iron and Steel's research on TRIP steel; it is a higher strength TRIP steel. Compared with other high-strength steels, the biggest feature of TRIP800 is that it has both high strength and high elongation, and can punch more complex parts; it also has high collision absorption performance. Once it encounters a collision, it will absorb energy through its own deformation instead of transmitting it to the outside. Therefore, it is often used in the fields of lightweight automobile bodies and rail transportation, such as automobile bumpers, chassis, A and B pillars and other anti-collision parts. 6061 aluminum alloy is widely used in various use conditions due to its manufacturability and excellent manufacturing performance. Because aluminum alloy has good mechanical properties, strong corrosion resistance, high weight-strength ratio and excellent formability, it is essential for weight reduction materials for transportation vehicles such as aircraft, automobiles, and high-speed railways, so it has wide application value in the automotive industry and rail transportation.

[0004] In recent years, with the continuous development of the world economy, the automobile manufacturing industry has become a pillar industry of the main economy of major industrial countries. However, the environmental problems brought about by the development of the automobile manufacturing industry and people's concerns about automobile safety have also received more attention. Nitrogen oxides, hydrocarbons, carbon monoxide and particulate matter (PM) emitted by automobiles have been confirmed to be one of the important sources of air pollution. Experts from the National Energy Commission have stated that automobile exhaust emissions have surpassed coal-fired pollution to become the main source of atmospheric pollution. Therefore, energy conservation and emission reduction, reduction of environmental pollution and improvement of safety have become the most important development goals of the modern automobile industry, and one of the important means to achieve this goal is to implement lightweight automobiles. In addition, whether it is a more mature fuel vehicle or an emerging new energy vehicle, in order to reduce energy consumption and improve endurance, lightweighting of the vehicle body is an inevitable trend for the next step of development. It is reported that for every 10% reduction in the weight of the whole vehicle, the fuel efficiency can be improved by 6% to 8%; and for every 100kg reduction in the weight of the spare parts of the whole vehicle, the fuel consumption per 100 kilometers can be reduced by 0.3 to 0.6L. Therefore, the lightweighting of automobiles has been strongly supported by the world's major automobile producing countries. Reducing the steel plate parts of automobiles that account for more than half of the weight of the vehicle body is one of the important ways to reduce the fuel consumption of automobiles. At the same time, the use of new aluminum alloys as automobile covering parts and body structural parts can effectively reduce the weight of the vehicle body. Using low-density high-strength alloys as automobile body materials to achieve lightweighting is a key development trend in the modern automobile manufacturing industry. TRIP high-strength steel with high strength and high elongation, as well as high collision absorption performance, can be used in many structural parts such as the A-pillar, B-pillar, front side beam, anti-collision beam, floor beam and wheels of the vehicle body. Therefore, TRIP high-strength steel and aluminum alloy are the preferred materials for automobile weight reduction, and the dissimilar material connection between these two materials has attracted widespread attention.

[0005] At present, the main problem in the welding of aluminum alloy / TRIP steel dissimilar metals is that the crystal structure and physical and chemical properties between aluminum and steel are very different. At room temperature, iron is almost not dissolved in aluminum, and brittle intermetallic compounds are very likely to appear at the welded joint. Steel-aluminum intermetallic compounds have two fatal weaknesses. One is that the material is brittle at low temperatures; the other is that when the temperature exceeds 600°C, the material strength and creep resistance drop sharply. Therefore, how to control the generation and size of the brittle and hard intermetallic compound layer is an urgent problem to be solved in the realization of laser welding of dissimilar metals between aluminum alloy and TIRP steel.

[0006] In order to solve the above problems, people have been seeking an ideal technical solution. Summary of the invention

[0007] The purpose of the present invention is to address the deficiencies in the prior art and to provide a TRIP steel-aluminum alloy laser welding method that can effectively suppress the excessive generation of brittle intermetallic compounds at the weld joint, optimize the mechanical properties of the weld joint, improve the connectivity of steel and aluminum dissimilar metals, and make the welding process simpler by adding a titanium / nickel composite intermediate layer.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is: a TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer, comprising the following steps:

[0009] Step S1, grinding, cleaning and drying the overlapping surfaces of the aluminum alloy sheet and the TRIP800 steel sheet to be welded to ensure that there is no metal oxide film, oil stain and moisture in the area to be welded;

[0010] Step S2, the aluminum alloy sheet is at the bottom and the TRIP800 steel sheet is at the top, and the two are overlapped horizontally, and a composite middle layer is sandwiched in the overlapped area, wherein the composite middle layer is composed of a pure nickel metal sheet at the bottom and a pure titanium metal sheet at the top;

[0011] Step S3, adjusting the motion path of the laser welding equipment and the preset weld to be on the same straight line, setting the welding parameters, and laser welding the overlapping area of ​​the aluminum alloy sheet and the TRIP800 steel sheet.

[0012] Based on the above, the laser spot radius is 1-2mm, the welding power is 1200W-1400W, the welding speed is 16mm / s-20mm / s, and the defocus is -1, 0 and +1.

[0013] Based on the above, the welding parameters in step S3 are: laser spot radius is 1 mm, welding power is 1300 W, welding speed is 18 mm / s, and defocus is 0.

[0014] Based on the above, in step S2, the thickness of the pure nickel metal sheet and the pure titanium metal sheet are both 0.05 mm and the purity is both 99.99%.

[0015] Based on the above, in step S2, a special fixture is used to clamp the aluminum alloy sheet and the TRIP800 steel sheet, and the special fixture includes a base, two pressing plates and a gasket. The top surface of the base is a flat structure with a groove in the center, and the two pressing plates are located on both sides of the groove. The base is provided with two studs at both ends of each pressing plate, and the pressing plate is provided with two through holes corresponding to the two studs. A nut for tightening the pressing plate is installed on each stud, and the thickness of the gasket is the same as that of the aluminum alloy sheet.

[0016] During the clamping process, the aluminum alloy sheet is directly placed on one side of the top surface of the base, and the side pressure plate presses the aluminum alloy sheet; the gasket is first placed on the other side of the top surface of the base, the TRIP800 steel sheet is placed on the gasket, and then the TRIP800 steel sheet is pressed by the side pressure plate to ensure that the TRIP800 steel sheet is horizontally overlapped; the weld in the overlapping area falls directly above the groove.

[0017] Based on the above, in step S2, the material of the gasket is TRIP800 steel.

[0018] Based on the above, step S1 includes the following sub-steps:

[0019] The surfaces of the overlapped areas of the aluminum alloy sheet and the TRIP800 steel sheet are polished using 800 mesh, 1500 mesh, and 2000 mesh sandpapers in sequence;

[0020] The polished aluminum alloy sheet and the TRIP800 steel sheet are placed in an ultrasonic cleaning apparatus for cleaning;

[0021] The aluminum alloy sheet and the TRIP800 steel sheet were taken out, their surfaces were cleaned with acetone, and they were blown dry with cold air from a hair dryer.

[0022] Based on the above, when the ultrasonic instrument cleaning device is used for cleaning, the solution is anhydrous ethanol, the cleaning time is 10 minutes, and the temperature is 25°C.

[0023] Based on the above, the chemical composition mass fraction percentage of the TRIP800 steel sheet is: C: 0.011; Si: 0.121; Mn: 0.155; P: 0.012; S: 0.004; Fe: balance;

[0024] The aluminum alloy thin plate is a 6061 aluminum alloy thin plate, and the chemical composition mass fraction percentage is: Mg: 1.09; Si: 0.65; Mn: 0.052; Fe: 0.56; Cr: 0.2; Zn: 0.01; Cu: 0.28; Ti: 0.019; Al: balance.

[0025] Based on the above, the thickness of the TRIP800 steel sheet is 1.2 mm, and the thickness of the aluminum alloy sheet is 2 mm.

[0026] The present invention has outstanding substantive features and significant progress compared to the prior art. Specifically, the present invention has the following advantages:

[0027] (1) The pure nickel metal sheet is in direct contact with the aluminum alloy sheet. Under the impact of the high energy density of the laser, the Ni element diffuses into the steel-aluminum welding joint to form a Ni-Al binary tough phase. At the same time, the pure nickel metal sheet can increase the diffusion degree of Fe in Al and inhibit the mass production of brittle intermetallic compounds at the interface. The pure titanium metal sheet is in direct contact with the TRIP800 steel sheet. In the molten state, Ti atoms will preferentially replace Al atoms in the FeAl compound to form a ductile FeAl alloy. 2 Ti compounds reduce the brittleness of the welded joint and improve the tensile shear properties of the welded joint; Ni-Al and Fe 2 Mixed tough phases such as Ti greatly inhibit the formation of brittle Fe-Al metal compounds, thereby greatly improving the mechanical properties of the welded joint.

[0028] According to experiments, the tensile shear performance of the weldment with the composite intermediate layer is improved by more than 35% compared with the weldment without the intermediate layer, more than 18% compared with the weldment with the pure nickel intermediate layer of the same thickness, and more than 22% compared with the weldment with the pure titanium intermediate layer of the same thickness.

[0029] (2) There is no spatter during the welding process, the weld is smooth and neat without collapse, the weldment is slightly deformed, the grain structure of the weld joint is fine, and the heat affected zone is narrow. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the clamping and welding of the aluminum alloy thin plate and the TRIP800 steel thin plate in the present invention.

[0031] Figure 2 It is a schematic diagram of the welding principle of the aluminum alloy thin plate and the TRIP800 steel thin plate in the present invention.

[0032] Figure 3 It is the surface image of the weld of the aluminum alloy thin plate and the TRIP800 steel thin plate welded by the method of the present invention.

[0033] Figure 4 It is a cross-sectional image of the weld of an aluminum alloy thin plate and a TRIP800 steel thin plate welded by the method of the present invention.

[0034] In the figure: 1. Aluminum alloy sheet; 2. TRIP800 steel sheet; 3. Base; 4. Pressure plate; 5. Gasket; 6. Groove; 7. Stud; 8. Nut; 9. Pure nickel metal sheet; 10. Pure titanium metal sheet; 11. Laser welding equipment; 12. Preset weld. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described in detail below through specific implementation methods.

[0036] like Figure 1 and Figure 2 As shown, the objects to be welded in this embodiment are an aluminum alloy thin plate 1 and a TRIP800 steel thin plate 2, wherein:

[0037] The aluminum alloy sheet 1 is a 6061 aluminum alloy sheet with dimensions of length×width×thickness=100×50×2 mm; the chemical composition mass fraction percentage is as follows: Mg: 1.09; Si: 0.65; Mn: 0.052; Fe: 0.56; Cr: 0.2; Zn: 0.01; Cu: 0.28; Ti: 0.019; Al: balance.

[0038] The dimensions of the TRIP800 steel sheet 2 are: length×width×thickness=100×50×1.2 mm; the chemical composition mass fraction percentages are: C: 0.011; Si: 0.121; Mn: 0.155; P: 0.012; S: 0.004; Fe: balance.

[0039] A special fixture is used for clamping, and the special fixture includes a base 3, two pressure plates 4 and a gasket 5. The top surface of the base 3 is a flat structure with a groove 6 in the center. The two pressure plates 4 are located on both sides of the groove 6. The base 3 is provided with two studs 7 at both ends of each pressure plate 4. The pressure plate 4 has two through holes corresponding to the two studs 7. Each of the studs 7 is installed with a nut 8 for tightening the pressure plate 4. The thickness of the gasket 5 is the same as that of the aluminum alloy sheet 1.

[0040] A TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer, comprising the following steps:

[0041] Step S1, pre-welding treatment, includes the following sub-steps:

[0042] The surfaces of the overlapped areas of the aluminum alloy sheet 1 and the TRIP800 steel sheet 2 are polished using 800 mesh, 1500 mesh, and 2000 mesh sandpapers in sequence to remove the metal oxide film, burrs, and oil stains on the surfaces;

[0043] The polished aluminum alloy sheet 1 and the TRIP800 steel sheet 2 are placed in an ultrasonic cleaning instrument for cleaning, the solution is anhydrous ethanol, the cleaning time is 10 minutes, the temperature is 25° C., and small stains on the surface are removed;

[0044] The aluminum alloy sheet 1 and the TRIP800 steel sheet 2 are taken out, and the residual ethanol on the surface is cleaned with acetone, and then dried with cold air from a hair dryer; ensuring that there is no metal oxide film, oil stain, or moisture in the overlapping area.

[0045] Step S2: using the special fixture to clamp the aluminum alloy sheet 1 and the TRIP800 steel sheet 2:

[0046] First, the aluminum alloy sheet 1 is directly placed on one side of the top surface of the base 3, and the side pressure plate 4 presses the aluminum alloy sheet 1 tightly;

[0047] A pure nickel metal sheet 9 is stacked on the upper surface of the overlapped area of ​​the aluminum alloy sheet 1, and a pure titanium metal sheet 10 is stacked on the upper surface of the pure nickel metal sheet 9. The thickness of the pure nickel metal sheet 9 and the pure titanium metal sheet 10 are both 0.05 mm and the purity is both 99.99%. The two together form a composite intermediate layer;

[0048] The gasket 5 is first placed on the other side of the top surface of the base 3, and the TRIP800 steel sheet 2 is placed on the gasket 5, and then the TRIP800 steel sheet 2 is pressed by the side pressing plate 4 to ensure that the TRIP800 steel sheet 2 is horizontally overlapped, so that the aluminum alloy sheet 1, the composite intermediate layer and the TRIP800 steel sheet 2 are in close contact, and the material of the gasket 5 is preferably TRIP800 steel to eliminate additional interference;

[0049] After the overlap is completed, the weld in the overlap area falls right above the groove 6 .

[0050] Step S3: Use laser welding equipment 11 to perform laser welding. The laser welding equipment is a YLR-2000-MM-WC fiber laser welder with a rated power range of 200W-2000W and a rated voltage of 230V:

[0051] Adjust the motion path of the laser welding device 11 and the preset weld 12 to be on the same straight line, set the welding parameters, and perform laser welding on the overlap area of ​​the aluminum alloy sheet 1 and the TRIP800 steel sheet 2;

[0052] The specific welding parameters can be: laser spot radius is 1-2mm, welding power is 1200W-1400W, welding speed is 16mm / s-20mm / s, defocus is -1, 0 and +1, the shielding gas used is inert gas argon with a purity of 99.99%, and the shielding gas flow rate is 15~20 L / min.

[0053] Preferably, the welding parameters are: laser spot radius is 1 mm, welding power is 1300 W, welding speed is 18 mm / s, and defocus is 0.

[0054] Laser deep melting welding is used in the welding method, so that the upper TRIP800 steel sheet 2 is completely melted, and the lower aluminum alloy sheet 1 is partially melted to form an elongated "nail head" shaped small hole molten pool. This welding method achieves high-quality connection of the TRIP800 steel sheet 2 and the aluminum alloy sheet 1. Figure 3 As shown in the figure, there is no spatter during welding, the weld is smooth and neat without collapse, and the weldment has little deformation; Figure 4 As shown in the figure, the weld joint has fine grain structure and narrow heat affected zone.

[0055] After experiments, the TRIP steel-aluminum alloy weldment made by the TRIP steel-aluminum alloy laser welding method with the addition of titanium / nickel composite intermediate layer can reach a tensile shear force of 1569.79 N in the tensile shear test. The applicant also conducted experiments on TRIP steel-aluminum alloy without adding an intermediate layer, using a 0.1 mm thick pure nickel metal sheet as an intermediate layer, and using a 0.1 mm thick pure titanium metal sheet as an intermediate layer under the same welding parameters and other welding conditions. The tensile shear performance of the three is 1140.57 N, 1312.62 N and 1263.23 N respectively. The welding method of this patent improves the shear resistance performance of the three by 37.632%, 19.592% and 24.268% respectively.

[0056] Working principle:

[0057] According to research, the use of the pure nickel metal sheet 9 and the pure titanium metal sheet 10 as the composite intermediate layer can effectively improve the mechanical properties of the lap joint. Specifically, the pure nickel metal sheet 9 is in direct contact with the aluminum alloy sheet 1. Under the impact of the high energy density of the laser, the Ni element diffuses into the steel-aluminum welding joint to form a Ni-Al binary tough phase. At the same time, the pure nickel metal sheet 9 can increase the diffusion degree of Fe in Al and inhibit the mass production of brittle intermetallic compounds at the interface. The pure titanium metal sheet 10 is in direct contact with the TRIP800 steel sheet 2. In the molten state, Ti atoms will preferentially replace Al atoms in the FeAl compound to form a ductile FeAl phase. 2 Ti compounds reduce the brittleness of the welded joint and improve the tensile shear properties of the welded joint; Ni-Al and Fe 2 Mixed tough phases such as Ti greatly inhibit the formation of brittle Fe-Al metal compounds, thereby greatly improving the mechanical properties of the welded joint.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A TRIP steel-aluminum alloy laser welding method with a titanium / nickel composite intermediate layer, characterized in that: The following steps are involved: Step S1, grinding, cleaning and drying the overlapping surfaces of the aluminum alloy sheet and the TRIP800 steel sheet to be welded to ensure that there is no metal oxide film, oil stain and moisture in the area to be welded, and the mass fraction percentage of the chemical composition of the TRIP800 steel sheet is: C: 0.011; Si: 0.121; Mn: 0.155; P: 0.012; S: 0.004; Fe: balance; The aluminum alloy sheet is a 6061 aluminum alloy sheet, and the chemical composition mass fraction percentage is: Mg: 1.09; Si: 0.65; Mn: 0.052; Fe: 0.56; Cr: 0.2; Zn: 0.01; Cu: 0.28; Ti: 0.019; Al: balance; The thickness of the TRIP800 steel sheet is 1.2 mm, and the thickness of the aluminum alloy sheet is 2 mm; Step S2: The aluminum alloy sheet is at the bottom and the TRIP800 steel sheet is at the top, and the two are overlapped horizontally, and a composite middle layer is sandwiched in the overlapped area, wherein the composite middle layer is composed of a lower layer of pure nickel metal sheet and an upper layer of pure titanium metal sheet, and the thickness of the pure nickel metal sheet and the pure titanium metal sheet are both 0.05 mm and the purity is both 99.99%. Step S3, adjust the movement path of the laser welding equipment and the preset weld to the same straight line, set the welding parameters, and perform laser welding on the overlapping area of ​​the aluminum alloy sheet and the TRIP800 steel sheet; the welding parameters in step S3 are: laser spot radius of 1-2mm, welding power of 1200W-1400W, welding speed of 16mm / s-20mm / s, defocus of -1, 0 and +1; the welding parameters in step S3 are: laser spot radius of 1mm, welding power of 1300W, welding speed of 18mm / s, defocus of 0; laser deep fusion welding is adopted in the welding method, so that the TRIP800 steel sheet of the upper layer is completely melted, and the aluminum alloy sheet of the lower layer is partially melted to form an elongated "nail head" shaped small hole molten pool.

2. The TRIP steel-aluminum alloy laser welding method with titanium / nickel composite intermediate layer added according to claim 1, characterized in that: In step S2, a special fixture is used to clamp the aluminum alloy sheet and the TRIP800 steel sheet. The special fixture includes a base, two pressing plates and a gasket. The top surface of the base is a flat structure with a groove in the center. The two pressing plates are located on both sides of the groove. The base is provided with two studs at both ends of each pressing plate. The pressing plate is provided with two through holes corresponding to the two studs. A nut for tightening the pressing plate is installed on each stud. The thickness of the gasket is the same as that of the aluminum alloy sheet. During the clamping process, the aluminum alloy sheet is directly placed on one side of the top surface of the base, and the side pressure plate presses the aluminum alloy sheet; the gasket is first placed on the other side of the top surface of the base, the TRIP800 steel sheet is placed on the gasket, and then the TRIP800 steel sheet is pressed by the side pressure plate to ensure that the TRIP800 steel sheet is horizontally overlapped; the weld in the overlapping area falls directly above the groove.

3. The TRIP steel-aluminum alloy laser welding method with titanium / nickel composite intermediate layer added according to claim 2, characterized in that: In step S2, the material of the gasket is TRIP800 steel.

4. The TRIP steel-aluminum alloy laser welding method with titanium / nickel composite intermediate layer added according to any one of claims 1 to 3, characterized in that: Step S1 includes the following sub-steps: The surfaces of the overlapped areas of the aluminum alloy sheet and the TRIP800 steel sheet are polished using 800 mesh, 1500 mesh, and 2000 mesh sandpapers in sequence; The polished aluminum alloy sheet and the TRIP800 steel sheet are placed in an ultrasonic cleaning apparatus for cleaning; The aluminum alloy sheet and the TRIP800 steel sheet were taken out, their surfaces were cleaned with acetone, and they were blown dry with cold air from a hair dryer.

5. The TRIP steel-aluminum alloy laser welding method with titanium / nickel composite intermediate layer added according to claim 4, characterized in that: When the ultrasonic instrument cleaning device is used for cleaning, the solution is anhydrous ethanol, the cleaning time is 10 minutes, and the temperature is 25°C.

Citation Information

Cited By

  • Intermediate steel alloy for joining dissimilar metals and uses thereof

    WO2026090485A1