A water-based cationic epoxy curing agent and preparation method thereof
The preparation of aqueous cationic epoxy curing agents through a series of reaction steps of ketone/aldehyde and polyethylene polyamines, solving the problems of poor storage stability and poor anti-corrosion performance of existing aqueous ionic epoxy curing agents, and achieving efficient aqueous rings Oxygen coating film anticorrosion performance and low cost production.
Patent Information
- Application Number
- CN202211646020.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-21
AI Technical Summary
The existing water-based ionic epoxy curing agent has poor storage stability and poor anti-corrosion performance of paint films formed by composite films with water-based epoxy resins, making it difficult to meet practical application requirements.
Small molecule ketone/aldehyde react with polyethylene polyamine to form secondary amine group intermediates, then react with epoxy group-containing compounds to form tertiary amine structure intermediates, and then react with acid solution to form primary amine group cationic epoxy The curing agent was prepared by capping and diluting the small molecule substances were removed by vacuum extraction to prepare an aqueous cationic epoxy curing agent.
The prepared aqueous cationic epoxy curing agent has excellent storage stability and anticorrosion properties of paint film formed by composite film with aqueous epoxy resin. It has a simple process and low production cost, making it suitable for large-scale industrial applications.
Smart Images

Figure BDA0004009406780000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy curing agents, and in particular to a water-based cationic epoxy curing agent and a preparation method thereof. Background Art
[0002] Waterborne epoxy resin uses water as solvent, which is safe and convenient to construct. It also meets environmental protection requirements and may completely replace traditional solvent-based epoxy resin in the future. At present, the commonly used curing agents for waterborne epoxy resin include waterborne non-ionic epoxy curing agents and waterborne ionic epoxy curing agents. Waterborne non-ionic epoxy curing agents have the advantages of good storage stability and excellent salt spray resistance of the paint film formed by compounding with waterborne epoxy resin, but their production cost is high and their application is greatly limited. The production cost of waterborne ionic epoxy curing agents is relatively low and has better practical application prospects. However, most of the existing waterborne ionic epoxy curing agents have problems such as poor storage stability and poor anti-corrosion performance of the paint film formed by compounding with waterborne epoxy resin, which makes it difficult to fully meet the requirements of practical applications.
[0003] Therefore, it is of great significance to develop a water-based cationic epoxy curing agent with simple preparation process, low production cost, good storage stability, and excellent anti-corrosion performance of the paint film formed by compounding with water-based epoxy resin.
[0004] The above statements merely provide background information related to the present invention and do not necessarily constitute prior art. Summary of the invention
[0005] The purpose of the present invention is to provide a water-based cationic epoxy curing agent and a preparation method thereof
[0006] The technical solution adopted by the present invention is:
[0007] A method for preparing a water-based cationic epoxy curing agent comprises the following steps:
[0008] 1) mixing a small molecule ketone / aldehyde and polyethylene polyamine to react to obtain an intermediate containing a secondary amine group;
[0009] 2) adding an excess of a compound containing an epoxy group to an intermediate containing a secondary amine group to react to obtain an intermediate containing a tertiary amine structure;
[0010] 3) adding a small molecule acid solution to the intermediate containing a tertiary amine structure to react to obtain a cationic epoxy curing agent containing a primary amine group;
[0011] 4) Partially cap the cationic epoxy curing agent containing primary amine groups, dilute with water, and then vacuum to remove small molecular ketones
[0012] / aldehyde to obtain a water-based cationic epoxy curing agent.
[0013] Preferably, the small molecule ketone in step 1) is at least one of acetone, butanone, methyl isobutyl ketone, cyclohexanone and isophorone.
[0014] Preferably, the small molecule aldehyde in step 1) is at least one of propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, isovaleraldehyde and pivalaldehyde.
[0015] Preferably, the polyethylene polyamine in step 1) is at least one of diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
[0016] Preferably, in step 1), the molar ratio of the small molecule ketone / aldehyde to the primary amine group in the polyethylene polyamine is 1.2-1.6:1.
[0017] Preferably, the reaction in step 1) is carried out at 70°C to 100°C, and the reaction time is 8h to 12h.
[0018] Preferably, the specific operation of step 1) is: mixing a small molecule ketone / aldehyde and polyethylene polyamine to react, and removing the water produced by the reaction in time during the reaction, and then performing a vacuum operation for 1h to 3h at a temperature of 100°C to 120°C and a vacuum degree of -0.10MPa to -0.06MPa (to remove excess small molecule ketone / aldehyde) to obtain an intermediate containing a secondary amine group.
[0019] Preferably, the epoxy group-containing compound in step 2) is at least one of monoglycidyl ether and a hydrophobic epoxy resin having a diepoxy group.
[0020] Preferably, the monoglycidyl ether is C1~C 14 At least one of alkyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether and cardanol glycidyl ether.
[0021] Preferably, the hydrophobic epoxy resin having a diepoxy group is at least one of epoxy resin E51, epoxy resin E44, and epoxy resin E20.
[0022] Preferably, in step 2), the molar ratio of the epoxy group in the epoxy group-containing compound to the secondary amine group in the secondary amine group-containing intermediate is 1.2 to 1.6:1.
[0023] Preferably, the reaction in step 2) is carried out at 70°C to 90°C, and the reaction time is 1h to 3h.
[0024] Preferably, the small molecule acid in the small molecule acid solution in step 3) is at least one of formic acid, acetic acid and propionic acid.
[0025] Preferably, in step 3), the molar ratio of the small molecule acid in the small molecule acid solution to the tertiary amine group in the intermediate containing a tertiary amine structure is 0.3 to 0.6:1.
[0026] Preferably, in step 3), the molar ratio of water in the small molecule acid solution to ketone / aldimine in the intermediate containing a tertiary amine structure is 2.2 to 3.0:1.
[0027] Preferably, the end-capping in step 4) is carried out at 70°C to 90°C, and the reaction time is 1h to 3h.
[0028] Preferably, the amount of water added in step 4) is 60% to 100% of the mass of the intermediate containing the tertiary amine structure.
[0029] Preferably, the temperature of the water in step 4) is 30°C to 60°C.
[0030] Preferably, the dilution with water in step 4) is carried out at a stirring speed of 500 r / min to 1500 r / min, and the stirring time is 20 min to 60 min.
[0031] Preferably, the specific operation of vacuuming to remove small molecule ketones / aldehydes in step 4) is: performing vacuuming operation for 1 h to 3 h at a temperature of 50° C. to 80° C. and a vacuum degree of -0.10 MPa to -0.06 MPa (to remove excess small molecule ketones / aldehydes).
[0032] A water-based cationic epoxy curing agent is prepared by the above preparation method.
[0033] The beneficial effects of the present invention are as follows: the paint film formed by compounding the water-based cationic epoxy curing agent of the present invention with the water-based epoxy resin has excellent anti-corrosion performance, and its preparation process is simple, the production cost is low, and the storage stability is good, and it is suitable for large-scale industrial application.
[0034] Specifically:
[0035] 1) The present invention is based on the primary amino group protection method, so that different amine hydrogens in polyethylene polyamine can effectively and selectively participate in the reaction (secondary amine groups only participate in tertiary amination and cationization reactions, and primary amine groups participate in blocking, unblocking, partial blocking and other reactions), thereby preparing a water-based cationic epoxy curing agent with excellent storage stability, and the paint film formed by compounding the water-based epoxy resin has excellent anti-corrosion performance, and can be applied in the field of water-based epoxy coatings;
[0036] 2) The raw materials of the water-based cationic epoxy curing agent of the present invention are cheap and easily available, the preparation cost is low, the process is simple, and it is suitable for large-scale industrial production. DETAILED DESCRIPTION
[0037] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0038] Embodiment 1:
[0039] A water-based cationic epoxy curing agent, the preparation method of which comprises the following steps:
[0040] 1) 216 g of isobutyraldehyde and 103 g of diethylenetriamine were mixed (the molar ratio of primary amine groups in isobutyraldehyde and diethylenetriamine was 1.5:1), and the mixture was reacted in a closed container at 70° C. for 8 h, and the water produced by the reaction was removed in time during the reaction. The mixture was then vacuumed for 1 h at a temperature of 100° C. and a vacuum degree of -0.08 MPa (to remove excess isobutyraldehyde), to obtain 211 g of a diethylenetriamine-based aldimine intermediate;
[0041] 2) adding 150 g of phenyl glycidyl ether and 170 g of benzyl glycidyl ether to the diethylenetriamine aldimine intermediate (the molar ratio of the epoxy groups in phenyl glycidyl ether and benzyl glycidyl ether to the secondary amine groups in the diethylenetriamine aldimine intermediate is 1.6:1), reacting at 70° C. for 3 h to obtain 531 g of the diethylenetriamine aldimine intermediate containing a tertiary amine structure;
[0042] 3) adding 73.2 g of 41% by mass acetic acid solution to the diethylenetriamine aldimine intermediate containing a tertiary amine structure (the molar ratio of acetic acid in the acetic acid solution to the tertiary amine group in the diethylenetriamine aldimine intermediate containing a tertiary amine structure is 0.5:1, and the molar ratio of water in the acetic acid solution to the aldimine in the diethylenetriamine aldimine intermediate containing a tertiary amine structure is 2.4:1), reacting at room temperature for 10 min to obtain a cationic epoxy curing agent containing a primary amine group;
[0043] 4) The cationic epoxy curing agent containing a primary amine group was heated to 70° C. and reacted for 3 h, then cooled to 30° C. and 531 g of deionized water was added (the amount of deionized water added was 100% of the mass of the diethylenetriamine-based aldimine intermediate containing a tertiary amine structure), the stirring speed was controlled to 500 r / min, stirred for 20 min, and then vacuumed for 3 h at a temperature of 50° C. and a vacuum degree of -0.08 MPa (to remove excess isobutyraldehyde and part of the deionized water), to obtain a water-based cationic epoxy curing agent.
[0044] Embodiment 2:
[0045] A water-based cationic epoxy curing agent, the preparation method of which comprises the following steps:
[0046] 1) 240 g of methyl isobutyl ketone and 146 g of triethylenetetramine were mixed (the molar ratio of the primary amine groups in methyl isobutyl ketone and triethylenetetramine was 1.2:1), and the mixture was reacted at 100° C. for 10 h in a closed state, and the water produced by the reaction was removed in time during the reaction. The mixture was then vacuumed for 2 h at a temperature of 120° C. and a vacuum degree of −0.09 MPa to obtain 510 g of a triethylenetetramine ketimine intermediate;
[0047] 2) adding 300 g of butyl glycidyl ether and 150 g of epoxy resin E51 to the triethylenetetramine ketimine intermediate (the molar ratio of the epoxy groups in butyl glycidyl ether and epoxy resin E51 to the secondary amine groups in the triethylenetetramine ketimine intermediate is 1.4:1), reacting at 80° C. for 2 h to obtain 960 g of the triethylenetetramine ketimine intermediate containing a tertiary amine structure;
[0048] 3) adding 105 g of a 56% propionic acid solution to a triethylenetetramine ketimine intermediate containing a tertiary amine structure (the molar ratio of propionic acid in the propionic acid solution to the tertiary amine group in the triethylenetetramine ketimine intermediate containing a tertiary amine structure is 0.4:1, and the molar ratio of water in the propionic acid solution to the aldimine in the triethylenetetramine ketimine intermediate containing a tertiary amine structure is 2.6:1), reacting at room temperature for 20 min to obtain a cationic epoxy curing agent containing a primary amine group;
[0049] 4) The cationic epoxy curing agent containing a primary amine group was heated to 80° C. and reacted for 2 h, then cooled to 40° C. and 768 g of deionized water was added (the amount of deionized water added was 80% of the mass of the triethylenetetramine ketimine intermediate containing a tertiary amine structure), the stirring speed was controlled to 800 r / min, stirred for 60 min, and then vacuumed for 2 h at a temperature of 60° C. and a vacuum degree of -0.09 MPa (to remove excess methyl isobutyl ketone and part of the deionized water), to obtain a water-based cationic epoxy curing agent.
[0050] Embodiment 3:
[0051] A water-based cationic epoxy curing agent, the preparation method of which comprises the following steps:
[0052] 1) 230 g of butanone and 189 g of tetraethylene pentamine were mixed (the molar ratio of butanone to the primary amine groups in tetraethylene pentamine was 1.6:1), and the mixture was reacted in a sealed container at 90° C. for 9 h, and the water produced by the reaction was removed in time during the reaction. The mixture was then vacuumed for 3 h at a temperature of 110° C. and a vacuum degree of −0.06 MPa to obtain 297 g of a tetraethylene pentamine ketimine intermediate;
[0053] 2) 150 g of butyl glycidyl ether, 240 g of octyl glycidyl ether, 280 g of dodecyl glycidyl ether and 140 g of epoxy resin E44 were added to the tetraethylene pentamine ketimine intermediate (the molar ratio of the epoxy groups in butyl glycidyl ether, octyl glycidyl ether, dodecyl glycidyl ether and epoxy resin E44 to the secondary amine groups in the tetraethylene pentamine ketimine intermediate was 1.2:1), and the reaction was carried out at 90° C. for 1 h to obtain 1107 g of the tetraethylene pentamine ketimine intermediate containing a tertiary amine structure;
[0054] 3) adding 137 g of a 60% by mass formic acid solution to a tetraethylene pentamine ketimine intermediate containing a tertiary amine structure (the molar ratio of formic acid in the formic acid solution to the tertiary amine group in the tetraethylene pentamine ketimine intermediate containing a tertiary amine structure is 0.6:1, and the molar ratio of water in the formic acid solution to the aldimine in the tetraethylene pentamine ketimine intermediate containing a tertiary amine structure is 3.0:1), reacting at room temperature for 30 min to obtain a cationic epoxy curing agent containing a primary amine group;
[0055] 4) The cationic epoxy curing agent containing a primary amine group was heated to 90° C. and reacted for 1 h, then cooled to 50° C. and 665 g of deionized water was added (the amount of deionized water added was 60% of the mass of the tetraethylenepentaminketimine intermediate containing a tertiary amine structure), the stirring speed was controlled to 1500 r / min, stirred for 40 min, and then vacuumed for 1 h at a temperature of 80° C. and a vacuum degree of -0.07 MPa (to remove excess butanone and part of the deionized water), to obtain a water-based cationic epoxy curing agent.
[0056] Embodiment 4:
[0057] A water-based cationic epoxy curing agent, the preparation method of which comprises the following steps:
[0058] 1) 240 g of pivalaldehyde, 31 g of diethylenetriamine and 102 g of triethylenetetramine were mixed (the molar ratio of pivalaldehyde to the primary amine groups in diethylenetriamine and triethylenetetramine was 1.4:1), and the mixture was reacted at 80° C. for 12 h, and the water produced by the reaction was removed in time during the reaction. The mixture was then vacuumed for 1 h at a temperature of 120° C. and a vacuum degree of -0.07 MPa to obtain 269 g of a mixed aldimine intermediate of diethylenetriamine and triethylenetetramine;
[0059] 2) 130 g of decyl glycidyl ether, 200 g of phenyl glycidyl ether, 80 g of cardanol glycidyl ether, 100 g of epoxy resin E51 and 100 g of epoxy resin E20 were added to a mixed aldimine intermediate of diethylenetriamine and triethylenetetramine (the molar ratio of the epoxy groups in decyl glycidyl ether, phenyl glycidyl ether, cardanol glycidyl ether, epoxy resin E51 and epoxy resin E20 to the secondary amine groups in the mixed aldimine intermediate of diethylenetriamine and triethylenetetramine was 1.5:1), and the mixture was reacted at 80° C. for 2.5 h to obtain 879 g of a mixed aldimine intermediate of diethylenetriamine and triethylenetetramine containing a tertiary amine structure;
[0060] 3) adding 70 g of 42% acetic acid solution to the mixed aldimine intermediate containing diethylenetriamine and triethylenetetramine with a tertiary amine structure (the molar ratio of acetic acid in the acetic acid solution to the tertiary amine group in the mixed aldimine intermediate containing diethylenetriamine and triethylenetetramine with a tertiary amine structure is 0.3:1, and the molar ratio of water in the acetic acid solution to the aldimine in the mixed aldimine intermediate containing diethylenetriamine and triethylenetetramine with a tertiary amine structure is 2.2:1), reacting at room temperature for 30 min to obtain a cationic epoxy curing agent containing a primary amine group;
[0061] 4) The cationic epoxy curing agent containing a primary amine group was heated to 80° C. and reacted for 2 h, then cooled to 60° C. and 615 g of deionized water was added (the amount of deionized water added was 70% of the mass of the mixed aldimine intermediate containing a tertiary amine structure of diethylenetriamine and triethylenetetramine), the stirring speed was controlled to 1100 r / min, stirred for 30 min, and then vacuumed for 3 h at a temperature of 70° C. and a vacuum degree of -0.06 MPa (to remove excess pivalaldehyde and part of the deionized water), to obtain a water-based cationic epoxy curing agent.
[0062] Performance Test:
[0063] The performance of the water-based cationic epoxy curing agent of Examples 1 to 4 was tested, and the test results are shown in the following table:
[0064] Table 1 Performance test results of water-based cationic epoxy curing agents of Examples 1 to 4
[0065]
[0066] Note:
[0067] Solid content: Tested in accordance with "GB 1725-1979 Determination of solid content of coatings";
[0068] Amine hydrogen equivalent: Tested in accordance with "GB / T 7383-2020 Determination of hydroxyl value of non-ionic surfactants";
[0069] Viscosity: Tested in accordance with "GB / T 22235-2008 Determination of Liquid Viscosity";
[0070] Adhesion: Tested in accordance with "GB / T 9286-2021 Paint and varnish cross-cut test";
[0071] Water resistance: Tested in accordance with "GB / T 4893.1-2005 Test method for resistance to cold liquid on furniture surface";
[0072] Hardness: Test according to "ASTM D3363-2000 Pencil Test for Determination of Paint Film Hardness";
[0073] Neutral salt spray resistance time: Tested in accordance with "GB / T 1771-1991 Determination of neutral salt spray resistance of paints and varnishes".
[0074] Preparation of paint film: The epoxy emulsion EP304 of Guangdong Huaguoshan Environmental Protection Technology Co., Ltd. was mixed evenly with the water-based cationic epoxy curing agent of Examples 1 to 4 according to the epoxy value and active hydrogen equivalent ratio of 1:0.8, and then sprayed on the sandblasted steel plate and cured at room temperature for 168 hours.
[0075] It can be seen from Table 1 that the water-based cationic epoxy curing agent of the present invention has good storage stability and can be stored at room temperature for more than half a year without obvious changes. The paint film formed by compounding it with the water-based epoxy resin has good water resistance, hardness F or above, strong adhesion (adhesion grade / hundred grid method is 0), and good salt spray resistance.
[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a water-based cationic epoxy curing agent, It is characterized in that The following steps are involved: 1) Mix small molecule ketone / aldehyde and polyethylene polyamine to react to obtain an intermediate containing a secondary amine group; 2) adding an excess of a compound containing an epoxy group to an intermediate containing a secondary amine group to react to obtain an intermediate containing a tertiary amine structure; 3) adding a small molecule acid solution to the intermediate containing a tertiary amine structure to react and obtain a cationic epoxy curing agent containing a primary amine group; 4) Partially cap the cationic epoxy curing agent containing primary amine groups, dilute with water, and then vacuum remove small molecular ketones / aldehydes to obtain a water-based cationic epoxy curing agent; Step 1) the small molecule ketone is at least one of acetone, butanone, methyl isobutyl ketone, cyclohexanone and isophorone; Step 1) the small molecule aldehyde is at least one of propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, isovaleraldehyde, and pivalaldehyde; Step 1) the polyethylene polyamine is at least one of diethylenetriamine, triethylenetetramine and tetraethylenepentamine; Step 2) the epoxy group-containing compound is at least one of monoglycidyl ether and a hydrophobic epoxy resin having a diepoxy group; The monoglycidyl ether is C 1 ~C 14 At least one of alkyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, and cardanol glycidyl ether; The hydrophobic epoxy resin having a diepoxy group is at least one of epoxy resin E51, epoxy resin E44, and epoxy resin E20; Step 3) the small molecule acid in the small molecule acid solution is at least one of formic acid, acetic acid, and propionic acid; Step 1) the molar ratio of the small molecule ketone / aldehyde to the primary amine group in the polyethylene polyamine is 1.2 to 1.6:1; Step 2) the molar ratio of the epoxy group in the epoxy group-containing compound to the secondary amine group in the secondary amine group-containing intermediate is 1.2 to 1.6:1; Step 3) The molar ratio of the small molecule acid in the small molecule acid solution to the tertiary amine group in the intermediate containing a tertiary amine structure is 0.3-0.6:
1.
2. The method for preparing the water-based cationic epoxy curing agent according to claim 1, Features: Step 1) The reaction is carried out at 70°C to 100°C for 8h to 12h.
3. The method for preparing the water-based cationic epoxy curing agent according to claim 1, Features: Step 2) The reaction is carried out at 70°C to 90°C for 1 h to 3 h.
4. The method for preparing the water-based cationic epoxy curing agent according to claim 1, Features: Step 3) The molar ratio of water in the small molecule acid solution to ketone / aldimine in the intermediate containing a tertiary amine structure is 2.2-3.0:
1.
5. The method for preparing the water-based cationic epoxy curing agent according to claim 1, Features: Step 4) The end-capping is carried out at 70°C to 90°C, and the reaction time is 1h to 3h.
6. A method for preparing a water-based cationic epoxy curing agent according to any one of claims 1, 4 and 5, Features: Step 4) The amount of water added is 60% to 100% of the mass of the intermediate containing the tertiary amine structure.
7. A water-based cationic epoxy curing agent, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Cited By
Cationic waterborne epoxy curing agent without containing free amine and preparation method of cationic waterborne epoxy curing agent
CN121005866A
Non-ionic waterborne epoxy curing agent without containing free amine and preparation method of non-ionic waterborne epoxy curing agent
CN121005867A
A free amine-free nonionic waterborne epoxy curing agent and a preparation method thereof
CN121005867B