An iron-nickel alloy with high magnetic permeability and low coercivity and its preparation method and application

By adjusting the elemental composition and process flow of iron-nickel alloys, high-purity alloys are prepared, which solves the problems of reduced mechanical properties of iron-nickel alloys after heat treatment and unstable magnetic properties under extremely weak magnetic fields, and achieves high magnetic permeability and low correction. Iron-nickel alloy with strong force and excellent mechanical properties, suitable for magnetic shielding barrel materials.

CN115948680BActive Publication Date: 2024-10-01NANJING DAMAI SCI&TECH IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310006983.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-10-01
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

The mechanical properties of existing iron-nickel alloys decrease after heat treatment, the magnetic shielding effect is weakened, and the magnetic properties are low and unstable under extremely weak magnetic fields, making it difficult to meet the requirements of good mechanical properties and magnetic properties at the same time.

Method used

By adjusting the Ni element content, adding Mo, Nb, Cr and other elements, using vacuum induction furnace smelting, forging, hot rolling, cold rolling and multi-pass cold rolling annealing, combined with inert gas protection and stress relief annealing, high-purity Alloys form a stable multi-phase structure to improve magnetic permeability and mechanical properties.

Benefits of technology

It achieves high magnetic permeability, low coercive force, high hardness, high strength and good high temperature oxidation resistance. It is suitable for magnetic shielding barrel materials. The magnetic permeability μ0.08≥150mH/m and the maximum magnetic permeability μm≥450mH /m, coercive force <0.4A/m, hardness HV0.2≥280, tensile strength ≥650MPa, elongation ≥20%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115948680B_ABST
    Figure CN115948680B_ABST
Patent Text Reader

Abstract

The invention discloses an iron-nickel alloy with high magnetic permeability and low coercivity, and a preparation method and application thereof. The raw materials of the iron-nickel alloy comprise the following components by weight percentage: Ni 80.6-81.2wt%, Mo 5.21-5.5wt%, Si≤0.03wt%, B 0.03-0.10wt%, Nb 0.04-0.10wt%, Cr 0.08-0.12%, C≤0.01wt%, S≤0.01wt%, P≤0.01wt%, and the balance is Fe and inevitable impurities. The preparation method comprises the following steps: (1) smelting the raw materials in a vacuum induction furnace to obtain an alloy ingot; (2) forging; (3) hot rolling; (4) cold rolling; and (5) obtaining a strip with a good plate shape by straightening, heating the strip to 530-630°C under the protection of an inert gas, and performing stress relief annealing at a speed of 10-20m / min. The iron-nickel alloy can be used in magnetic shielding combination barrels. The present invention uses iron-nickel as the matrix and achieves excellent mechanical properties and magnetic properties through compounding of different element contents. The material prepared by the present invention has high magnetic permeability, low coercivity, high hardness and high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an alloy and a preparation method thereof, in particular to a high-purity alloy with high magnetic permeability and low coercivity and a preparation method and application thereof. Background Art

[0002] Fe-Ni soft magnetic alloy is a kind of alloy with high magnetic permeability and low coercivity in weak magnetic field. It shows high magnetic permeability and low coercivity under weak magnetic field magnetization, and has good cold working performance. By changing the content of the composition, adding one or several alloy elements (such as Mo, Cu, Cr and Ti, etc.) and regulating the process, a variety of Permalloys with different characteristics can be obtained. Its variety is the most among soft magnetic materials. This type of alloy is widely used in radio electronics industry, precision instruments and meters, remote control and automatic control systems. It is mainly used in energy conversion and information processing. It is an important material in the national economy.

[0003] At present, the soft magnetic properties of iron-nickel alloys include initial magnetic permeability, maximum magnetic permeability, coercive force, etc. The magnetic shielding barrel requires the coercive force to be as low as possible, and the initial magnetic permeability and maximum magnetic permeability to be as high as possible. The use of magnetic shielding barrels requires sufficient strength and AC magnetic properties, and must be heat treated to adjust the performance. Therefore, it is necessary to select multi-element alloys with high nickel content to ensure magnetic properties on the one hand and mechanical properties on the other hand. It is extremely difficult to ensure the magnetic properties and mechanical properties of alloy materials at the same time. The currently used Permalloy includes alloy materials such as 1J85 and 1J79, whose magnetic properties can basically meet the use requirements. However, after being made into magnetic shielding barrels, their mechanical properties will decrease during heat treatment, which will lead to easy deformation and weakened magnetic shielding effect. In addition, under extremely weak magnetic field strength, the magnetic properties of alloy materials such as 1J85 and 1J79 are low and unstable, which limits the use of magnetic shielding barrels under extremely weak magnetic fields. Therefore, materials that have good mechanical and magnetic properties at the same time and still maintain good magnetic properties under extremely weak magnetic fields have good development prospects in the application field of magnetic shielding barrels. Summary of the invention

[0004] Purpose of the invention: The present invention aims to provide an iron-nickel alloy with high magnetic permeability and low coercivity having excellent mechanical properties and magnetic properties, and the present invention also provides a preparation method and application of the iron-nickel alloy.

[0005] Technical solution: The iron-nickel alloy with high magnetic permeability and low coercivity described in the present invention comprises the following components in weight percentage: Ni 80.6-81.2wt%, Mo 5.21-5.5wt%, Si≤0.03wt%, B0.03-0.10wt%, Nb 0.04-0.10wt%, Cr 0.08-0.12%, C≤0.01wt%, S≤0.01wt%, P≤0.01wt%, and the balance is Fe and unavoidable impurities.

[0006] Furthermore, the contents of Nb, B and Cr meet the following conditions: Nb+B+Cr≤0.3wt%, and the sum of the contents of Nb, B and Cr is not greater than 0.3wt%, which can effectively deoxidize and desulfurize, reduce the gas content of the alloy, improve the microstructure of the alloy, and improve the strength and magnetic properties.

[0007] The method for preparing the iron-nickel alloy with high magnetic permeability and low coercivity of the present invention comprises the following steps:

[0008] (1) The raw materials are smelted in a vacuum induction furnace to obtain alloy ingots;

[0009] (2) Forging: forging into forging blanks at 1280-1320°C for 1-1.5 hours;

[0010] (3) Hot rolling: hot rolling at 1260-1300°C for 30-60 minutes to form hot-rolled billets;

[0011] (4) Cold rolling: multiple cold rolling and intermediate annealing are performed to form finished strip;

[0012] (5) The strip with good plate shape is obtained by straightening, and the temperature is raised to 530-630°C under the protection of inert gas, and stress relief annealing is performed at a speed of 10-20m / min.

[0013] Furthermore, in step (2), the thickness of the forged billet is 50-90 mm and the width is 300-600 mm; in step (3), the thickness of the hot-rolled billet is 5-8 mm and the width is 300-600 mm; in step (4), the total deformation rate of the cold rolling is controlled at 60%-75%, and the cold rolling deformation rate of the finished product is controlled at 70-80%. The intermediate annealing treatment is specifically as follows: under hydrogen protection conditions, the temperature is raised to 950-1080°C, and continuous annealing treatment is performed at a speed of 1.5-5.5 m / min. The thickness of the finished strip is 0.5-2 mm and the width is 300-600 mm.

[0014] The invention discloses an application of the high magnetic permeability and low coercive force iron-nickel alloy in a magnetic shielding composite barrel.

[0015] Furthermore, the magnetic shielding barrel is a rectangular barrel or a circular barrel.

[0016] Furthermore, the combination of the rectangular barrels is as follows:

[0017] The first layer consists of a rectangular barrel of A*B and a lid of (A+δ)*(B+δ)mm. A The round hole in the barrel is reused The enameled wire is wound along the middle and lower parts of the barrel to make 80-100 turns of coils, and then fixed with insulating paint;

[0018] The second layer consists of a rectangular barrel of C*D and a lid of (C+δ)*(D+δ)mm. A hole is punched on the lid 10-15mm away from the center. The round hole in the barrel is reused The enameled wire is wound along the middle and lower parts of the barrel for 60-80 turns, and then fixed with insulating paint;

[0019] The third layer consists of a rectangular barrel of E*F and a lid of (E+δ)*(F+δ)mm. A hole is punched on the lid 15-20mm away from the center. Circular holes;

[0020] The fourth layer consists of a rectangular barrel of G*H and a lid of (G+δ)*(H+δ)mm. A hole is punched on the lid 20-25mm away from the center. Circular holes;

[0021] Insulating foam is used to isolate the layers; A and B are ≤400mm; the gap between the layers is between 10-25mm; δ is the wall thickness of the alloy material, and δ is between 0.5-2.0mm.

[0022] Furthermore, the combination of the circular barrels is as follows:

[0023] The first layer consists of a round barrel of D1 and a lid of D1+δmm. A The round hole in the barrel is reused The enameled wire is wound vertically from the bottom of the barrel to the barrel mouth with 6-8 turns of coil, and fixed with insulating material;

[0024] The second layer consists of a round barrel of D2 and a lid of D2+δmm. A hole is punched on the lid 10-15mm off the center. Circular holes;

[0025] The third layer consists of a D3 round barrel and a D3+δmm lid. A hole is punched on the lid 15-20mm off the center. Circular holes;

[0026] The fourth layer consists of a D4 round barrel and a D4+δmm lid. A hole is punched on the lid 20-25mm off the center. Circular holes;

[0027] Insulating foam is used to isolate the layers, wherein D1≤300mm; the gap between the layers is between 10-25mm; δ is the wall thickness of the alloy material, and δ is between 0.5-2.0mm.

[0028] Principle of the invention: The present invention uses iron-nickel as the matrix, reasonably controls the Ni content, slightly exceeds the content of traditional materials, discards the Mn element, and adds the main alloy element Mo and the secondary B, Nb, and Cr elements. Through the compounding of different element contents, the material composition design of excellent mechanical properties and magnetic properties is achieved at the same time. The high-purity alloy material prepared by the present invention has high magnetic permeability, low coercivity, high hardness, and high strength.

[0029] The influence of the alloying elements of the present invention on the alloy is as follows:

[0030] Ni: makes the alloy have high magnetic permeability, and too low a content will increase the coercive force of the alloy, so the Ni content is preferably 80.6-81.2%.

[0031] Mo, Nb, Cr: During the heat treatment of the iron-nickel binary alloy, when it passes through high temperature to room temperature, the entire structure will form Ni3Fe during the cooling process, and a long-range ordered change will occur, which significantly reduces the lattice constant and magnetic properties of the alloy material. Adding Mo, Nb, and Cr elements can inhibit the formation of Ni3Fe and slow down the change rate of the long-range order of Ni3Fe during the heat treatment, thereby gaining more time and temperature range for heat treatment regulation. Among them, the addition of trace amounts of Nb and Cr elements to the alloy can promote the formation of a solid solution phase of the Mo element and exist in the matrix together with it, and the Nb, Cr, and Mo elements can have a solid solution strengthening effect on the γ-Fe phase or γ'-Fe phase, and form a cubic texture to obtain a stable multiphase structure, so that the magnetocrystalline anisotropy constant K1 and the magnetostriction coefficient λ1 of the alloy material are infinitely close to zero after heat treatment, thereby greatly improving the magnetic permeability of the alloy material. Adding different amounts of Nb and Mo reacts with the carbon element in the alloy to form stable primary carbides or secondary carbides, which can reduce the supersaturation of the matrix and precipitate Mo2C and Mo6C, which are dispersed at the grain boundaries of the alloy, thereby improving the stability of the organization and thus the strength of the alloy.

[0032] B: Adding element B can improve the high temperature oxidation resistance of the alloy. At the same time, the addition of B also brings the technical effect of improving the tensile strength and elongation of the alloy material. B can also form two nanophases of boron nitride and boron carbide with nitrogen and carbon in the alloy, and improve the strength of the alloy material through uniform dispersion precipitation.

[0033] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0034] (1) The present invention adds Mo, B, Nb, and Cr elements, removes Mn elements, and effectively controls the gas content and purity of the alloy by smelting in a vacuum furnace and adding trace alloy elements. The hardness, strength, and magnetic energy of the alloy are improved by forging, hot rolling, cold rolling, and reasonable heat treatment.

[0035] (2) The alloy prepared by the present invention has a magnetic permeability μ0.08≥150mH / m, a maximum magnetic permeability μm≥450mH / m, a coercive force <0.4A / m, a hardness HV0.2≥280, a tensile strength ≥650MPa, an elongation ≥20%, and an average grain size >200μm after heat treatment at a magnetic field strength of 0.08A / m.

[0036] (3) The present invention combines the composition ratio of materials with process conditions to design a high-purity alloy strip that has excellent mechanical properties and magnetic properties and can be used to prepare materials for magnetic shielding barrels. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a wiring diagram of the bottom end of the magnetic shielding barrel of the present invention;

[0038] Figure 2 This is a diagram of the overall wiring method of the magnetic shielding barrel of the present invention;

[0039] Figure 3 This is a wiring diagram of the magnetic shielding barrel connected to the degaussing machine of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below in conjunction with embodiments and drawings.

[0041] Embodiment 1: The raw materials of the iron-nickel alloy with high magnetic permeability and low coercivity described in the present invention have the following components, measured in weight percentage: Ni 81.2wt%, Mo 5.5wt%, Si≤0.03wt%, B 0.08wt%, Nb 0.04wt%, Cr0.08%, C≤0.01wt%, S≤0.01wt%, P≤0.01wt%, and the balance is Fe and unavoidable impurities.

[0042] The preparation method of the above-mentioned iron-nickel alloy comprises the following steps:

[0043] (1) The raw materials are smelted in a vacuum induction furnace to obtain alloy ingots;

[0044] (2) Forging: at 1320°C, keep warm for 1.5 hours, and forge into a forging billet with a thickness of 90 mm and a width of 500 mm;

[0045] (3) Hot rolling: hot rolling at 1300°C for 60 minutes into a hot-rolled billet with a thickness of 5 mm and a width of 500 mm;

[0046] (4) Cold rolling: multiple cold rolling and intermediate annealing treatments are performed, the total deformation rate of cold rolling is controlled at 70%, and the cold rolling deformation rate of the finished product is controlled at 70%. The intermediate annealing treatment is specifically as follows: under hydrogen protection conditions, the temperature is raised to 950-1080°C, and continuous annealing treatment is performed at a speed of 1.5-5.5 m / min to roll into a finished strip with a thickness of 0.75 mm and a width of 500 mm;

[0047] (5) The strip with good plate shape is obtained by straightening, and the temperature is raised to 630°C under the protection of inert gas, and stress relief annealing is carried out at a speed of 15m / min.

[0048] Embodiment 2: The raw materials of the iron-nickel alloy with high magnetic permeability and low coercivity described in the present invention have the following components, measured in weight percentage: Ni 80.6wt%, Mo 5.25wt%, Si≤0.03wt%, B 0.1wt%, Nb 0.1wt%, Cr0.12%, C≤0.01wt%, S≤0.01wt%, P≤0.01wt%, and the balance is Fe and unavoidable impurities.

[0049] The preparation method of the above-mentioned iron-nickel alloy comprises the following steps:

[0050] (1) The raw materials are smelted in a vacuum induction furnace to obtain alloy ingots;

[0051] (2) Forging: at 1300°C, keep warm for 1.5 hours, and forge into a forging billet with a thickness of 90 mm and a width of 500 mm;

[0052] (3) Hot rolling: hot rolling at 1290°C for 60 minutes into a hot-rolled billet with a thickness of 5 mm and a width of 500 mm;

[0053] (4) Cold rolling: multiple cold rolling and intermediate annealing treatments are performed, the total deformation rate of cold rolling is controlled at 70%, and the cold rolling deformation rate of the finished product is controlled at 70%. The intermediate annealing treatment is specifically as follows: under hydrogen protection conditions, the temperature is raised to 950-1080°C, and continuous annealing treatment is performed at a speed of 1.5-5.5 m / min to roll into a finished strip with a thickness of 0.75 mm and a width of 500 mm;

[0054] (5) The strip with good plate shape is obtained by straightening, and the temperature is raised to 630°C under the protection of inert gas, and stress relief annealing is carried out at a speed of 15m / min.

[0055] Comparative Example 1: Conventional Permalloy material 1J85, in terms of weight percentage, has the following components: Ni 80wt%, Mo 5.0wt%, Si 0.12wt%, Mn 0.50wt%, C ≤ 0.01wt%, S ≤ 0.01wt%, P ≤ 0.01wt%, and the balance is Fe and unavoidable impurities.

[0056] The preparation method of the above-mentioned iron-nickel alloy comprises the following steps:

[0057] (1) The raw materials are smelted in a vacuum induction furnace to obtain alloy ingots;

[0058] (2) Forging: forging at 1280°C for 1.5 hours into a forging blank with a thickness of 90 mm and a width of 500 mm;

[0059] (3) Hot rolling: hot rolling at 1260°C for 60 minutes into a hot-rolled billet with a thickness of 5 mm and a width of 500 mm;

[0060] (4) Cold rolling: multiple cold rolling and intermediate annealing treatments are performed, the total deformation rate of cold rolling is controlled at 70%, and the cold rolling deformation rate of the finished product is controlled at 70%. The intermediate annealing treatment is specifically as follows: under hydrogen protection conditions, the temperature is raised to 950-1080°C, and continuous annealing treatment is performed at a speed of 1.5-5.5 m / min to roll into a finished strip with a thickness of 0.75 mm and a width of 500 mm;

[0061] (5) The strip with good plate shape is obtained by straightening, and the temperature is raised to 630°C under the protection of inert gas, and stress relief annealing is carried out at a speed of 15m / min.

[0062] Example 3: The alloy materials of Example 1, Example 2 and the comparative example are combined into a magnetic shielding barrel according to the combination method of the magnetic shielding barrel circular barrel of the present invention. The specific combination method is as follows:

[0063] The first layer consists of a round barrel of D1 and a lid of D1+δmm. A The round hole in the barrel is reused The enameled wire is wound vertically from the bottom of the barrel to the barrel mouth with 6-8 turns of coil, and fixed with insulating material;

[0064] The second layer consists of a round barrel of D2 and a lid of D2+δmm. A hole is punched on the lid 10-15mm off the center. Circular holes;

[0065] The third layer consists of a D3 round barrel and a D3+δmm lid. A hole is punched on the lid 15-20mm off the center. Circular holes;

[0066] The fourth layer consists of a D4 round barrel and a D4+δmm lid. A hole is punched on the lid 20-25mm off the center. Circular holes;

[0067] Insulating foam is used to isolate the layers, wherein D1≤300mm; the gap between the layers is between 10-25mm; δ is the wall thickness of the alloy material, and δ is between 0.5-2.0mm.

[0068] The demagnetization process is an overall demagnetization, that is, the 4 layers of Permalloy are a whole (the aluminum layer does not require demagnetization winding and punching), and a hole is opened at the bottom away from the center for the overall demagnetization routing. The demagnetization line reaches the bottom along the outer wall, passes through the demagnetization routing hole, turns 60°, and then passes through the inner wall, circulating 6 times in sequence to form an overall current loop. During the design process, it is necessary to shorten the connecting line at the outer end of the inner and outer walls and make it into an intersecting head. It is usually laid out on the outer and inner walls without interfering with the normal opening and closing of the barrel cover. During the demagnetization process, they are connected separately according to the line sequence to form an overall current loop for demagnetization.

[0069] Figure 1 The left picture shows the rear end view of the shield barrel, and the right picture shows the wiring method of a group of wires.

[0070] Figure 2 The outermost layer of Permalloy and the innermost layer of Permalloy are included.

[0071] Figure 1 The left picture requires a circle that deviates from the axis of the cylinder to pass the wire. All four layers of Permalloy need to have an eccentric circle, but the aluminum layer does not. Figure 2 For the convenience of drawing, there is no eccentric circle.

[0072] Figure 1 Middle: The same serial number refers to the same wire, 6 in total.

[0073] Figure 2 In the example, the current wiring method is as follows Figure 3 shown.

[0074] The test data of the alloy materials are shown in Table 1, Table 2, and Table 3, and the magnetic shielding test data of the magnetic shielding barrel is shown in Table 4.

[0075] Table 1 Oxygen, hydrogen, nitrogen content and material purity of alloy samples after heat treatment

[0076] Oxygen content ppm Hydrogen content ppm Nitrogen content ppm purity% Example 1 10 15 20 99.998 Example 2 11 16 29 99.998 Comparative Example 1 20 26 45 99.992

[0077] Table 2 Magnetic properties of finished alloy samples after heat treatment

[0078]

[0079] Table 3 Mechanical properties of finished alloy samples after heat treatment

[0080] Tensile strength MPa Elongation % Hardness Hv0.2 Average grain size μm Example 1 718 31 297 270 Example 2 702 28 289 256 Comparative Example 1 614 26 245 280

[0081] Table 4 Magnetic shielding test data of magnetic shielding pain after demagnetization

[0082] Electromagnetic field inside the shielding barrel nT Example 1 4 Example 2 5 Comparative Example 1 15

Claims

1. Application of an iron-nickel alloy with high magnetic permeability and low coercivity in a magnetic shielding combination barrel, characterized in that: The iron-nickel alloy comprises the following components by weight percentage: Ni 80.6-81.2wt%, Mo 5.21-5.5%wt%, Si≤0.03wt%, B 0.03-0.10wt%, Nb 0.04-0.10wt%, Cr 0.08-0.12%, C≤0.01wt%, S≤0.01wt%, P≤0.01wt%, and the balance is Fe and unavoidable impurities; the contents of Nb, B and Cr meet the following conditions: Nb+B+Cr≤0.3wt%; The preparation method of the iron-nickel alloy comprises the following steps: (1) The raw materials are smelted in a vacuum induction furnace to obtain alloy ingots; (2) Forging: forging into forging blanks at 1280-1320℃ for 1-1.5 hours; (3) Hot rolling: hot rolling at 1260-1300℃ for 30-60 minutes into hot-rolled billet; (4) Cold rolling: multiple cold rolling and intermediate annealing are performed to form finished strip; (5) The strip with good plate shape is obtained by straightening, and the temperature is raised to 530-630°C under the protection of inert gas, and stress relief annealing is performed at a speed of 10-20m / min; In step (2), the thickness of the forging blank is 50-90 mm and the width is 300-600 mm; In step (3), the hot-rolled billet has a thickness of 5-8 mm and a width of 300-600 mm; In step (4), the finished strip obtained after the intermediate annealing treatment has a thickness of 0.5-2 mm and a width of 300-600 mm; The iron-nickel alloy, after heat treatment, has a magnetic permeability μ0.08≥150mH / m at a magnetic field strength of 0.08A / m, a maximum magnetic permeability μm≥450mH / m, a coercive force <0.4A / m, a hardness HV0.2≥280, a tensile strength ≥650MPa, an elongation ≥20%, and an average grain size >200μm; The magnetic shielding barrel is a rectangular barrel or a circular barrel; the combination of the rectangular barrel is as follows: The first layer consists of a rectangular barrel of A*B and a lid of (A+δ)*(B+δ) mm. A circular hole of φ20-30 mm is punched in the center of the lid. The barrel is then wound with φ0.9 mm enameled wire along the upper and lower middle parts of the barrel to form 80-100 turns of coils, which are then fixed with insulating paint. The second layer is composed of a rectangular barrel of C*D and a lid of (C+δ)*(D+δ) mm. A circular hole of φ20-30 mm is punched on the lid at a position 10-15 mm away from the center. The barrel body is then wound with φ0.9 mm enameled wire along the middle and lower parts of the barrel body for 60-80 turns of coils, and then fixed with insulating paint. The third layer consists of a rectangular barrel of E*F and a lid of (E+δ)*(F+δ) mm, with a circular hole of φ20-30 mm punched in the lid at a position 15-20 mm off the center; The fourth layer consists of a rectangular barrel of G*H and a lid of (G+δ)*(H+δ) mm, with a circular hole of φ20-30 mm punched on the lid at a position 20-25 mm off the center; Insulating foam is used to isolate the layers; A and B are ≤ 400 mm; the gap between the layers is between 10 and 25 mm; δ is the wall thickness of the iron-nickel alloy, and δ is between 0.5 and 2.0 mm; The combination of the circular barrels is as follows: The first layer consists of a round barrel of D1 and a lid of D1+δmm. A φ20-30mm round hole is punched in the center of the lid. A φ2mm enameled wire is used to wind 6-8 turns of coils vertically from the bottom of the barrel to the barrel mouth, and fixed with insulating materials. The second layer consists of a round barrel of D2 and a lid of D2+δmm, with a circular hole of φ20-30mm punched in the lid at a position 10-15mm off the center; The third layer consists of a D3 round barrel and a D3+δmm lid, with a φ20-30mm round hole punched in the lid 15-20mm off the center. The fourth layer is composed of a D4 round barrel and a D4+δmm lid, with a φ20-30mm round hole punched in the lid at a position 20-25mm off the center; Insulating foam is used to isolate the layers, wherein D1≤300mm; the gap between the layers is between 10-25mm; δ is the wall thickness of the iron-nickel alloy, and δ is between 0.5-2.0mm.

2. The use according to claim 1, characterized in that: In step (4), the total deformation rate of cold rolling is controlled at 60%-75%, and the deformation rate of finished product cold rolling is controlled at 70-80%. The intermediate annealing treatment is specifically: under hydrogen protection conditions, the temperature is raised to 950-1080°C and continuous annealing treatment is performed at a speed of 1.5-5.5m / min.