A catalytic cracking catalyst containing phosphate waste residue and preparation method thereof
Catalytic cracking catalyst is prepared by combining the phosphate waste residue treated with the mother liquor of SAPO molecular sieve, binder and clay, which solves the problems of resource waste and environmental pollution, reduces production costs, and improves the cracking performance of the catalyst.
Patent Information
- Application Number
- CN202111174848.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-09
AI Technical Summary
The phosphate waste residue generated during the production of SAPO molecular sieve cannot be effectively utilized, resulting in environmental pollution and waste of resources. At the same time, the production cost of catalytic cracking catalysts is high, and the existing technology is difficult to effectively reduce.
The phosphate waste residue treated with the mother liquor of SAPO molecular sieve is used to prepare a catalytic cracking catalyst. By combining it with molecular sieve, binder, clay, etc., a catalyst with modified metal oxide is formed, and the catalyst is prepared by spray molding and calcination.
The recycling of SAPO molecular sieve mother liquor wastewater is realized, the production cost of catalytic cracking catalysts is reduced, the heavy oil cracking capacity and coke selectivity of the catalyst are improved, and environmental pollution is reduced.
Smart Images

Figure BDA0003294984680000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of oil refining catalysts. The present invention relates to a catalytic cracking catalyst and a preparation method thereof, and in particular, to a catalytic cracking catalyst comprising phosphate waste residue, wherein the phosphate waste residue is derived from SAPO molecular sieve mother liquor wastewater, and further relates to a method for preparing the catalytic cracking catalyst by using SAPO molecular sieve mother liquor wastewater. Background Art
[0002] Silicoaluminophosphate molecular sieve (SAPO) plays an important role in the field of heterogeneous catalysis due to its unique properties. For example, it is used in methanol to olefins catalysts to increase the selectivity of light olefins, and in selective catalytic reduction catalysts (NO X -SCR) reduces NO X At present, the industrial production of SAPO series molecular sieves mainly adopts the hydrothermal crystallization method, which is to mix water, aluminum source, phosphorus source, silicon source and template agent and other raw materials in a certain order, stir them evenly into a sol state, and then place them in a crystallization kettle with a set temperature for crystallization to form a molecular sieve slurry, and then obtain the molecular sieve product through solid-liquid separation and drying.
[0003] However, in the solid-liquid separation process of SAPO molecular sieve slurry, a large amount of mother liquor wastewater containing elements such as phosphorus, aluminum, silicon and organic templates will be generated. If it is directly discharged without treatment, it will harm the environment and also lead to the waste of useful resources such as phosphorus, aluminum and silicon. At present, the treatment of SAPO molecular sieve mother liquor wastewater mainly focuses on several aspects: first, improving the recycling of organic templates, second, strengthening the resource utilization of phosphate waste residues, and third, the mother liquor is directly reused as a raw material in the preparation of molecular sieves or catalysts. Common methods for treating SAPO molecular sieve mother liquor include: using incineration treatment method, after treatment, the organic amines in the recovered wastewater can be reused in the synthesis of SAPO molecular sieves, and the enriched and recovered phosphates can be used as raw materials for the phosphate industry; using chemical precipitation method, that is, adding a certain amount of certain metal salts or polymers to the wastewater, so that the dissolved phosphate in the sewage forms insoluble salts and precipitates.
[0004] CN105314757A discloses a method for treating SAPO molecular sieve crystallization mother liquor wastewater, which adopts an inorganic polymer composite flocculant to remove ions such as Al, Si, and P from SAPO molecular sieve crystallization mother liquor wastewater containing high ion concentration, adds alkali to the deionized wastewater to adjust the pH value so that the organic amine is oleaginized and released from the wastewater, and the organic amine is separated by an oil-water separator and reused for SAPO molecular sieve synthesis.
[0005] CN109092353A discloses a method for preparing a propylene production-increasing auxiliary agent, comprising the following steps: (1) removing a template agent from a SAPO molecular sieve synthesis mother liquor to obtain a refined mother liquor; (2) mixing the refined mother liquor, a carrier, a ZSM-5 molecular sieve and water to form a slurry, and spraying and solidifying the slurry to obtain a propylene production-increasing auxiliary agent.
[0006] The catalytic cracking unit is the main unit in my country's oil refining industry. Under high temperature, the catalytic cracking catalyst is used to crack heavy oil and convert it into products such as cracked gas, gasoline and diesel. Due to the large number of applications of catalytic cracking catalysts, researchers in this field have been committed to seeking effective methods to control their costs, hoping to obtain a catalytic cracking catalyst with easy-to-obtain raw materials, simple preparation process, effective production cost reduction, and good heavy oil conversion performance.
[0007] To this end, the present invention proposes to use the phosphate waste residue obtained after treating the SAPO molecular sieve mother liquor for the production of catalytic cracking catalyst, thereby realizing the recycling of SAPO molecular sieve mother liquor wastewater, solving the problems of environmental pollution and resource waste, and effectively reducing the production cost of the catalytic cracking catalyst. The catalytic cracking catalyst containing the phosphate waste residue prepared by using the SAPO molecular sieve mother liquor wastewater has good heavy oil cracking ability. Summary of the invention
[0008] On the one hand, the present invention provides a catalytic cracking catalyst comprising phosphate waste residue, wherein the catalytic cracking catalyst contains, based on the dry weight of the catalytic cracking catalyst, 10 to 50 weight % of molecular sieve, 10 to 50 weight % of clay, 5 to 40 weight % of binder and 1 to 30 weight % of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater, wherein, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 1 to 30 weight % of Al2O3, 30 to 80 weight % of P2O5, 1 to 10 weight % of SiO2 and 5 to 40 weight % of modified metal oxide, and the modified metal oxide is an oxide containing one or more metals selected from Mg, RE, Ti and Zr.
[0009] In one embodiment, the catalytic cracking catalyst according to the present invention contains, based on the dry weight of the catalytic cracking catalyst, 25-45 wt% of molecular sieve, 15-40 wt% of clay, 5-35 wt% of binder and 5-25 wt% of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater.
[0010] In one embodiment, according to the catalytic cracking catalyst of the present invention, the phosphate waste residue contains 2 to 20 weight % of Al2O3, 35 to 75 weight % of P2O5, 1 to 8 weight % of SiO2 and 10 to 30 weight % of modified metal oxide based on its dry weight.
[0011] In one embodiment, according to the catalytic cracking catalyst of the present invention, the molecular sieve is selected from one or more of Y-type molecular sieve, MFI shape selective molecular sieve, Beta-type molecular sieve, MCM molecular sieve, aluminum phosphate molecular sieve, and silicoaluminophosphate molecular sieve, preferably Y-type molecular sieve, and the Y-type molecular sieve can be selected from one or more of ultra-stable Y-type molecular sieve, Y-type molecular sieve containing phosphorus and / or rare earth metals, and ultra-stable Y-type molecular sieve containing phosphorus and / or rare earth metals.
[0012] In one embodiment, the catalytic cracking catalyst contains Y-type molecular sieve and optional other molecular sieves, wherein the other molecular sieves are one or more of MFI shape-selective molecular sieves, Beta-type molecular sieves, MCM molecular sieves, aluminum phosphate molecular sieves, and silicoaluminophosphate molecular sieves. Based on the dry weight of the catalytic cracking catalyst, the catalytic cracking catalyst contains 10 to 50% by weight, such as 10-45% by weight, of the Y-type molecular sieve and no more than 20% by weight, such as 0-15% by weight, of other molecular sieves.
[0013] In one embodiment, according to the catalytic cracking catalyst of the present invention, the clay is selected from one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth, and synthetic clay, preferably one or more of kaolin, metakaolin, and diatomaceous earth, preferably one or more of aluminum sol, silica sol, silica-aluminum composite sol, aluminum phosphate sol, and acidified pseudo-boehmite.
[0014] In one embodiment, according to the catalytic cracking catalyst of the present invention, the SAPO molecular sieve mother liquor wastewater can be selected from one or more of the liquids obtained after solid-liquid separation when preparing SAPO molecular sieves having a six-membered ring, eight-membered ring, ten-membered ring, or twelve-membered ring structure.
[0015] On the other hand, the present invention provides a method for preparing the above-mentioned catalytic cracking catalyst using SAPO molecular sieve mother liquor wastewater, the method comprising:
[0016] Step (1) mixing SAPO molecular sieve mother liquor wastewater and a compound containing a modified metal, adjusting the pH value of the mixed slurry to 5 to 10, reacting the mixed slurry at 20 to 90° C. for 30 to 120 minutes, and then evaporating and drying the mixed slurry to obtain phosphate waste residue; and
[0017] Step (2) The phosphate waste residue is mixed with a molecular sieve, a binder, clay and water to form a slurry, and the slurry is spray-formed and calcined to obtain the catalytic cracking catalyst containing the phosphate waste residue.
[0018] In one embodiment, according to the preparation method of the present invention, based on the dry weight of the phosphate waste residue, 60-95% of the SAPO molecular sieve mother liquor wastewater and 5-40% of the modified metal compound are mixed to obtain the phosphate waste residue. For example, the SAPO molecular sieve mother liquor wastewater and the modified metal compound can be mixed in a ratio of 60-95:5-40 on a dry basis to obtain the phosphate waste residue.
[0019] In one embodiment, according to the preparation method of the present invention, based on the dry weight of the catalyst, 1 to 30 wt% of the phosphate waste residue, 10 to 50 wt% of the molecular sieve, 5 to 40 wt% of the binder, and 10 to 50 wt% of the clay are mixed to form a slurry with a solid content of 10 to 50 wt%, and the slurry is spray-formed and calcined to obtain the catalytic cracking catalyst containing the phosphate waste residue.
[0020] In one embodiment, according to the preparation method of the present invention, the modified metal is one or more of Mg, RE, Ti, and Zr.
[0021] In the preparation method of the present invention, the SAPO molecular sieve mother liquor wastewater, molecular sieve, binder and clay used are as described above for the catalytic cracking catalyst of the present invention.
[0022] The beneficial effects of the present invention are as follows:
[0023] The invention provides a new use of SAPO molecular sieve mother liquor, solves the problem of utilizing a large amount of waste residue generated in the production process of SAPO molecular sieve, reduces the production cost of the molecular sieve, reduces the emission of hazardous wastes, and simultaneously uses the phosphate waste residue obtained after treating the SAPO molecular sieve mother liquor as an effective component of a catalytic cracking catalyst to replace part of the raw materials, thereby realizing the transformation of waste into treasure and significantly reducing the production cost of the catalytic cracking catalyst.
[0024] According to the present invention, the phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor can adjust the acidity and activity of the catalytic cracking catalyst to a certain extent, and can accommodate more coke on the matrix, avoid the damage to the molecular sieve, and improve the coke selectivity; at the same time, the mother liquor also contains a small amount of SAPO molecular sieve crystals, which are applied to the catalytic cracking catalyst to improve the selectivity of propylene to a certain extent. DETAILED DESCRIPTION
[0025] The specific embodiments of the present invention are described in detail below, wherein the technical features involved in different embodiments can be combined with each other as long as they do not conflict with each other. It should be understood that the specific embodiments described herein are intended to illustrate and explain the present invention, and do not constitute any limitation to the present invention.
[0026] On one hand, the present invention provides a catalytic cracking catalyst comprising phosphate waste residue. Based on the dry weight of the catalytic cracking catalyst, the catalytic cracking catalyst contains 10-50 wt% of molecular sieve, 10-50 wt% of clay, 5-40 wt% of binder and 1-30 wt% of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater. Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 1-30 wt% of Al2O3, 30-80 wt% of P2O5, 1-10 wt% of SiO2 and 5-40 wt% of modified metal oxide, and the modified metal oxide is an oxide containing one or more metals selected from Mg, RE, Ti and Zr. Among them, RE refers to rare earth metals, namely lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), scandium (Sc) and yttrium (Y).
[0027] According to a preferred embodiment of the present invention, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 2 to 20 weight % of Al2O3, 35 to 75 weight % of P2O5, 1 to 8 weight % of SiO2 and 10 to 30 weight % of modified metal oxides.
[0028] According to the present invention, the molecular sieve can be selected from one or more of a Y-type molecular sieve, an MFI shape-selective molecular sieve, a Beta-type molecular sieve, an MCM molecular sieve, an aluminum phosphate molecular sieve, and a silicon aluminum phosphate molecular sieve, preferably a Y-type molecular sieve. The Y-type molecular sieve can be selected from one or more of an ultra-stable Y-type molecular sieve, a Y-type molecular sieve containing phosphorus and / or a rare earth metal, and an ultra-stable Y-type molecular sieve containing phosphorus and / or a rare earth metal.
[0029] According to the present invention, the clay may be, for example, one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth, and synthetic clay, wherein one or more of kaolin, metakaolin, and diatomaceous earth are preferred.
[0030] According to the present invention, the binder can be selected from one or more of aluminum sol, silica sol, silica-aluminum composite sol, aluminum phosphate sol and acidified pseudo-boehmite. The binder can be purchased from a commercial source or prepared according to an existing method. For example, the acidified pseudo-boehmite can be prepared according to the method provided by patents US4010116 and US4206085. Preferably, the molar ratio of acid to pseudo-boehmite (in terms of alumina) when the pseudo-boehmite is acidified is 0.12 to 0.18. The aluminum phosphate sol can be prepared according to the method provided by patents CN1008974C and CN1083512A. The silica sol can be prepared according to the method provided by US Patents US3957689 and US3867308.
[0031] According to the present invention, the SAPO molecular sieve mother liquor wastewater can be selected from one or more of the liquids obtained after solid-liquid separation when preparing SAPO molecular sieves having six-membered rings, eight-membered rings, ten-membered rings or ten-membered wrinkled rings or twelve-membered rings.
[0032] The catalytic cracking catalyst of the present invention contains phosphate waste residue, which provides a green way for the effective utilization of the mother liquor wastewater generated in the preparation process of SAPO molecular sieve, reduces environmental pollution and waste of resources, and greatly reduces the production cost of the catalytic cracking catalyst. In addition, in combination with the subsequent embodiments, it can be seen that compared with conventional catalytic cracking catalysts, the catalytic cracking catalyst comprising the phosphate waste residue of the present invention has excellent heavy oil cracking ability, and the phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor contains rich phosphorus and modified metal components, which are added to the catalytic cracking catalyst, and the acidity and activity of the catalytic cracking catalyst are adjusted to a certain extent, and the coke selectivity is improved. At the same time, the mother liquor also contains a small amount of SAPO molecular sieve crystals, which are applied to the catalytic cracking catalyst to improve the selectivity of propylene to a certain extent.
[0033] Another aspect of the present invention provides a method for preparing the above-mentioned catalytic cracking catalyst using SAPO molecular sieve mother liquor wastewater, the method comprising:
[0034] Step (1) mixing SAPO molecular sieve mother liquor wastewater and a compound containing a modified metal, adjusting the pH value of the obtained mixed slurry to 5 to 10, preferably 6 to 9, reacting the mixed slurry at 20 to 90° C. for 30 to 120 minutes, and then evaporating and drying the mixed slurry to obtain phosphate waste residue; and
[0035] Step (2) The phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater is mixed with molecular sieve, binder, water and clay to form a slurry, and the slurry is spray-dried and calcined to obtain the catalytic cracking catalyst of the present invention as described above.
[0036] According to the preparation method of the present invention, in step (1), the SAPO molecular sieve mother liquor wastewater used to prepare the phosphate waste residue can be selected from one or more of the liquids obtained after solid-liquid separation when preparing SAPO molecular sieves with a six-membered ring, eight-membered ring, ten-membered ring, or twelve-membered ring structure. The SAPO molecular sieve having a six-membered ring structure may be one or more of SAPO-20, SAPO-25, and SAPO-28; the SAPO molecular sieve having an eight-membered ring structure may be one or more of SAPO-17, SAPO-18, SAPO-26, SAPO-33, SAPO-34, SAPO-35, SAPO-39, SAPO-42, SAPO-43, SAPO-44, and SAPO-47; the SAPO molecular sieve having a ten-membered ring structure may be one or more of SAPO-11, SAPO-31, and SAPO-41; the SAPO molecular sieve having a twelve-membered ring structure may be one or more of SAPO-5, SAPO-36, SAPO-37, SAPO-40, and SAPO-46.
[0037] The modified metal used in step (1) is selected from one or more of Mg, RE, Ti, and Zr. The Mg compound may be selected from one or more of magnesium oxide, magnesium carbonate, magnesium hydroxide, magnesium chloride, magnesium sulfate, and magnesium nitrate; RE is a rare earth metal, and the RE compound may be selected from one or more of rare earth oxides, rare earth carbonates, rare earth chlorides, and rare earth nitrates; the Ti compound may be selected from one or more of titanium oxide, titanium sulfate, titanium oxysulfate, titanium tetrachloride, titanium trichloride, tetrabutyl titanate, ammonium fluorotitanate, and titanium hydroxide; the Zr compound may be selected from one or more of zirconium oxide, zirconium hydroxide, zirconium tetrachloride, zirconium sulfate, zirconium nitrate, zirconium oxychloride, zirconium acetate, and zirconium isopropoxide.
[0038] In addition, in step (1), based on the dry weight of the phosphate waste residue, preferably 60 to 95 wt % of the SAPO molecular sieve mother liquor wastewater is mixed with 5 to 40 wt % of the modified metal compound to obtain the phosphate waste residue, wherein the phosphate waste residue contains 1 to 30 wt % of Al2O3, 30 to 80 wt % of P2O5, 1 to 10 wt % of SiO2 and 5 to 40 wt % of the modified metal oxide based on its dry weight. Depending on the above-mentioned modified metal compound used, the modified metal oxide can be an oxide containing one or more metals selected from Mg, RE, Ti and Zr.
[0039] According to the preparation method of the present invention, in step (2), based on the dry catalyst, preferably 1 to 30 wt% of the phosphate waste residue, 10 to 50 wt% of the molecular sieve, 5 to 40 wt% of the binder, and 10 to 50 wt% of the clay are mixed to form a slurry with a solid content of 10 to 50 wt% to obtain the catalytic cracking catalyst containing the phosphate waste residue. The molecular sieve, clay and binder used are as described above for the first aspect of the present invention and will not be repeated here.
[0040] In step (2), the phosphate waste residue obtained in step (1) can be mixed with clay and water to obtain a first slurry; the first slurry, a binder and a Y-type molecular sieve are mixed to obtain a second slurry, and the obtained second slurry is spray-dried and calcined. There is no particular limitation on the mixing and slurrying time, for example, it can be 30 to 120 minutes.
[0041] In addition, in step (1), the evaporation can be carried out by an evaporation device familiar to those skilled in the art, such as a single-effect evaporator or a multiple-effect evaporator, a concentrating evaporator, a falling film evaporation, or by reduced pressure dehydration, vacuum drying, etc. The purpose of evaporation is to remove the organic template contained in the mother liquor wastewater and recycle it. Drying can be carried out by constant temperature drying, airflow drying, spray drying, vacuum drying, freeze drying, etc., which are familiar to those skilled in the art. The purpose of drying is to remove the residual organic matter in the phosphate waste residue. The drying temperature can be 80 to 300°C, preferably 100 to 250°C, and the time can be selected according to actual needs, and there is no specific restriction on this.
[0042] In step (2), the spray drying is a technique known to those skilled in the art. The preparation of catalytic cracking catalysts generally adopts spray forming drying, and the temperature of the spray tail gas is controlled at 100-250°C. The roasting treatment is also well known to those skilled in the art. For example, it can be carried out in a muffle furnace. The roasting treatment conditions can be as follows: the temperature is 350-800°C, preferably 400-650°C, and the roasting time is 0.5-6 hours, preferably 1-4 hours; the roasting can be carried out in any atmosphere, such as air or an inert atmosphere. The inert atmosphere contains an inert gas, and the inert gas may include nitrogen, helium, argon, etc.
[0043] Example
[0044] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0045] The raw materials used in the following examples are composed as follows:
[0046] SAPO molecular sieve mother liquor wastewater comes from the mother liquor wastewater generated in the production of SAPO molecular sieves. The ICP element analysis results are as follows: P content 28000u / g, Al content 7800ug / g, Si content 700ug / g, solid content 14 weight%;
[0047] Kaolin was produced by Suzhou Kaolin Company with a solid content of 76% by weight;
[0048] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62.0 wt%;
[0049] The acidified aluminum stone is prepared by mixing pseudo-boehmite and hydrochloric acid, wherein the mass ratio of 36% hydrochloric acid to aluminum oxide is 0.20, and the solid content is 12.0% by weight;
[0050] The aluminum oxide content in the aluminum sol is 21.5% by weight;
[0051] Hydrochloric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 36%;
[0052] The solid content of rare earth ultrastable Y molecular sieve REUSY is 84.8% by weight, and the unit cell constant is In terms of weight percentage, the Na2O content is 1.6% and the RE2O3 content is 12.0%;
[0053] The solid content of ultrastable Y molecular sieve USY is 94.7% by weight, and the unit cell constant is In terms of weight percentage, the Na2O content is 1.3%;
[0054] ZSM-5 molecular sieve, SiO2 / Al2O3=40-50, Na2O content 3.5%, solid content 75 wt%;
[0055] Rare earth ultrastable Y molecular sieve REUSY, ultrastable Y molecular sieve USY and ZSM-5 molecular sieve are all produced by Sinopec Catalyst Co., Ltd., and the remaining reagents are produced by Sinopharm Chemical Reagent Co., Ltd., and all specifications are analytical grade.
[0056] The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics of the United States was used, and the low-temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2 Pa, vacuum degassing at 300 ° C for 4 h, using N2 as the adsorption medium, and measuring the adsorption-desorption isotherm of the sample at 77.4 K. The specific surface area (SBET) of the sample was calculated according to the BET formula, and the volume of N2 adsorbed by the sample at the relative pressure p / p0 = 0.98 was measured and converted into liquid nitrogen volume, i.e., pore volume;
[0057] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF).
[0058] The following Examples 1 to 4 are examples of preparing phosphate waste residue contained in the catalytic cracking catalyst of the present invention.
[0059] Example 1
[0060] 1000 g of SAPO molecular sieve mother liquor wastewater and 48 g of magnesium chloride were weighed and mixed, the slurry pH was adjusted to 9.5, and the mixed slurry was reacted at 25° C. for 60 min; then the mixed slurry was evaporated and dried to obtain phosphate waste residue A1, which contained 16.2 wt % of Al2O3, 69.6 wt % of P2O5, 1.7 wt % of SiO2 and 12.5 wt % of MgO on a dry basis.
[0061] Example 2
[0062] 1000 g of SAPO molecular sieve mother liquor wastewater and 118 ml of 270 g / l RECl3 solution were weighed and mixed, the slurry pH was adjusted to 9.0, and the mixed slurry was reacted at 40°C for 90 min; then the mixed slurry was evaporated and dried to obtain phosphate waste residue A2, which contained 15.1 wt% of Al2O3, 64.8 wt% of P2O5, 1.5 wt% of SiO2 and 18.6 wt% of rare earth oxides on a dry basis.
[0063] Example 3
[0064] 1000 g of SAPO molecular sieve mother liquor wastewater and 73 g of zirconium oxychloride were weighed and mixed, the slurry pH was adjusted to 10.0, and the mixed slurry was reacted at room temperature for 120 min; then the mixed slurry was evaporated and dried to obtain phosphate waste residue A3, which contained 15.5 wt% of Al2O3, 66.3 wt% of P2O5, 1.6 wt% of SiO2 and 16.7 wt% of zirconium oxide on a dry basis.
[0065] Example 4
[0066] 1000 g of SAPO molecular sieve mother liquor wastewater and 83 g of titanium tetrachloride were weighed and mixed, the slurry pH was adjusted to 8.5, and the mixed slurry was reacted at room temperature for 60 min; then the mixed slurry was evaporated and dried to obtain phosphate waste residue A4, which contained 14.8 wt% of Al2O3, 63.7 wt% of P2O5, 1.5 wt% of SiO2 and 20 wt% of titanium oxide on a dry basis.
[0067] The following Examples 5 to 8 are examples of preparing the catalytic cracking catalysts of the present invention, and Comparative Example 1 is an example of preparing a comparative catalytic cracking catalyst.
[0068] Example 5
[0069] 171 g of kaolin, 50 g of phosphate waste A1 and 779 g of deionized water were mixed in a slurrying tank and slurried for 60 min, then 833 g of aluminum oxide and 186 g of aluminum sol were added, and slurrying was continued for 30 min. Finally, 212 g of REUSY molecular sieve and 302 g of deionized water were added to form a slurry, stirred for 30 min, and then the obtained slurry was spray-dried and formed, and calcined at 500° C. for 2 hours to obtain the catalytic cracking catalyst C1 of the present invention.
[0070] Embodiments 6 to 8
[0071] Catalytic cracking catalysts C2-C4 were prepared by the same method as in Example 5, except that in Examples 6-8, the phosphate waste residue A1 in Example 5 was replaced by the same amount of phosphate waste residue A2-A4, respectively.
[0072] Comparative Example 1
[0073] Preparation of catalytic cracking catalyst DC1 free of phosphate waste residue.
[0074] 237 g of kaolin and 763 g of deionized water were mixed in a slurrying tank and slurried for 60 minutes. Then, 833 g of aluminum oxide and 186 g of aluminum sol were added and slurrying was continued for 30 minutes. Finally, 212 g of REUSY molecular sieve and 302 g of deionized water were added to form a slurry, stirred for 30 minutes, and then the obtained slurry was spray-dried and formed, and calcined at 500°C for 2 hours to obtain a comparative catalytic cracking catalyst DC1.
[0075] Table 1 Composition of catalysts C1 to C4 obtained in Examples 5 to 8 and catalyst DC1 obtained in Comparative Example 1
[0076] Example 5 Example 6 Example 7 Example 8 Comparative Example 1 Catalyst No. C1 C2 C3 C4 DC1 Kaolin, weight % 26 26 26 26 36 REUSY, weight % 36 36 36 36 36 Aluminite, weight % 20 20 20 20 20 Aluminum sol, weight % 8 8 8 8 8 Phosphate waste residue, weight % 10 10 10 10 0 total 100 100 100 100 100
[0077] Catalysts C1-C4 and DC1 were pre-aged at 800°C and 100% steam for 17 hours in a fixed bed aging device and then evaluated on an ACE device. The properties of the reaction raw oil are shown in Table 2. The reaction temperature was 500°C and the catalyst-oil weight ratio was 8.04.
[0078] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield; coke selectivity = coke yield / conversion rate. The evaluation results are shown in Table 3.
[0079] Table 2 Raw oil properties
[0080]
[0081] Table 3 Evaluation results
[0082] Example 5 Example 6 Example 7 Example 8 Comparative Example 1 catalyst C1 C2 C3 C4 DC1 Product distribution, weight % Dry gas 1.42 1.39 1.55 1.40 1.45 Liquefied gas 13.60 13.53 13.02 13.70 12.37 gasoline 42.07 43.81 43.91 42.65 40.96 diesel fuel 17.55 17.01 18.52 18.87 19.11 heavy oil 19.89 18.69 17.73 18.21 20.16 Coke 5.47 5.56 5.27 5.17 5.94 Conversion rate, weight % 62.56 64.29 63.75 62.92 60.72 Coke selectivity, % 8.74 8.65 8.27 8.22 9.78 Propylene yield, weight % 4.55 4.73 4.65 4.79 3.57 Liquefied gas propylene concentration, % 33.5 35.0 35.7 35.0 28.9
[0083] The results in Table 3 show that, compared with the catalyst without phosphate waste residue in Comparative Example 1, the catalytic cracking catalysts C1 to C4 of the present invention prepared by adding phosphate waste residue prepared in Examples 1 to 4 in Examples 5 to 8 have improved conversion, reduced heavy oil yield, increased liquefied gas yield, increased propylene yield and propylene concentration in liquefied gas, and improved coke selectivity. It can be seen that the phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater is suitable for direct use in the preparation of catalytic cracking catalysts.
[0084] Example 9
[0085] 204 g of kaolin, 25 g of phosphate waste residue A1 and 671 g of deionized water were mixed in a slurrying tank and slurried for 60 minutes; then 174 g of USY zeolite, 33 g of ZSM-5 and 335 g of deionized water were added to form a slurry, and after stirring for 30 minutes, 140 g of aluminum sol and 833 g of acidified aluminum stone were added, and the mixture was homogenized (stirred) for 30 minutes. Then, the obtained slurry was spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking catalyst C5 provided by the present invention. The catalyst composition is shown in Table 4.
[0086] Embodiments 10 to 12
[0087] The cracking catalysts C6-C8 of the present invention were prepared according to the method of Example 9. The catalyst compositions are shown in Table 4.
[0088] Comparative Example 2
[0089] According to the method of Example 9, a catalytic cracking catalyst DC2 free of phosphate waste residue was prepared.
[0090] Table 4 Catalyst composition
[0091] Example 9 Example 10 Embodiment 11 Example 12 Comparative Example 2 Catalyst No. C5 C6 C7 C8 DC2 Kaolin, weight % 31 26 21 16 36 Molecular sieve, weight % 38 38 38 38 38 Binder, weight % 26 26 26 26 26 Phosphate waste residue, weight % 5 10 15 20 / Types of phosphate waste A1 A2 A3 A4 / total 100 100 100 100 100
[0092] The catalytic cracking catalysts C5-C8 of Examples 9-12 and the comparative catalyst DC2 were pre-aged at 800°C and 100% steam for 12 hours in a fixed bed aging device, and then evaluated on an ACE device. The properties of the reaction raw oil are shown in Table 2 above. The reaction temperature was 500°C, the catalyst-oil weight ratio was 4.02, and the evaluation results are shown in Table 5.
[0093] Table 5 Evaluation results
[0094] Example 9 Example 10 Embodiment 11 Example 12 Comparative Example 2 catalyst C5 C6 C7 C8 DC2 Product distribution, weight % Dry gas 1.77 2.30 1.72 1.79 2.04 Liquefied gas 20.22 21.70 23.35 23.26 19.82 gasoline 45.82 44.13 43.02 42.79 45.07 diesel fuel 15.92 15.73 16.49 16.09 15.88 heavy oil 9.63 9.74 8.71 9.37 9.94 Coke 6.64 6.40 6.71 6.70 7.25 Conversion rate, weight % 74.45 74.53 74.80 74.54 74.18 Coke selectivity, % 8.92 8.59 8.97 8.99 9.77 Propylene yield, weight % 7.12 7.93 8.59 8.46 6.36 Liquefied gas propylene concentration, % 35.21 36.54 36.79 36.37 32.09
[0095] From the results in Table 5, it can be seen that compared with Comparative Example 2, the catalysts C5 to C8 containing phosphate waste residues prepared in Examples 9 to 12 of the present invention have improved conversion rates, reduced heavy oil yields, increased total liquid yields, improved coke selectivity, and increased propylene selectivity, which indicates that the catalytic cracking catalyst containing phosphate waste residues has a strong heavy oil cracking ability, improved coke selectivity, and increased propylene selectivity. And compared with catalysts C5 and C6, with the increase in the amount of phosphate waste residue added, the liquefied gas yield and propylene yield of catalysts C7 and C8 increase.
[0096] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A catalytic cracking catalyst comprising phosphate waste residue, wherein the catalytic cracking catalyst comprises, based on the dry weight of the catalytic cracking catalyst, 10 to 50 wt% of a molecular sieve, 10 to 50 wt% of a clay, 5 to 40 wt% of a binder and 1 to 30 wt% of a phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater; Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 1-30 wt % of Al2O3, 30-80 wt % of P2O5, 1-10 wt % of SiO2 and 5-40 wt % of modified metal oxide, wherein the modified metal oxide is an oxide containing one or more metals selected from Mg, RE, Ti and Zr; The preparation method of the phosphate waste residue comprises: The SAPO molecular sieve mother liquor wastewater and the compound containing the modified metal are mixed, the pH value of the mixed slurry is adjusted to 5-10, the mixed slurry is reacted at 20-90° C. for 30-120 minutes, and then evaporated and dried to obtain phosphate waste residue.
2. The catalytic cracking catalyst according to claim 1, wherein The catalytic cracking catalyst contains 25-45 wt % of molecular sieve, 15-40 wt % of clay, 5-35 wt % of binder and 5-25 wt % of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater.
3. The catalytic cracking catalyst according to claim 1 or 2, wherein: The phosphate waste residue contains 2-20 wt % of Al2O3, 35-75 wt % of P2O5, 1-8 wt % of SiO2 and 10-30 wt % of modified metal oxide.
4. The catalytic cracking catalyst according to claim 1, wherein The molecular sieve is selected from one or more of Y-type molecular sieve, MFI shape-selective molecular sieve, Beta-type molecular sieve, MCM molecular sieve, aluminum phosphate molecular sieve, and silicon aluminum phosphate molecular sieve, and the binder is selected from one or more of aluminum sol, silica sol, silicon aluminum composite sol, aluminum phosphate sol and acidified pseudo-boehmite.
5. The catalytic cracking catalyst according to claim 4, wherein The molecular sieve is a Y-type molecular sieve, which is selected from one or more of an ultra-stable Y-type molecular sieve, a Y-type molecular sieve containing phosphorus and / or rare earth metals, and an ultra-stable Y-type molecular sieve containing phosphorus and / or rare earth metals.
6. The catalytic cracking catalyst according to claim 1, wherein The clay is selected from one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.
7. The catalytic cracking catalyst according to claim 1, wherein The clay is one or more selected from kaolin, metakaolin and diatomaceous earth.
8. The catalytic cracking catalyst according to claim 1, wherein The SAPO molecular sieve mother liquor wastewater is selected from one or more of the liquids obtained after solid-liquid separation when preparing SAPO molecular sieves having a six-membered ring, an eight-membered ring, a ten-membered ring, or a twelve-membered ring structure.
9. A method for preparing the catalytic cracking catalyst according to any one of the preceding claims using SAPO molecular sieve mother liquor wastewater, the method comprising: Step (1) mixing SAPO molecular sieve mother liquor wastewater and a compound containing a modified metal, adjusting the pH value of the mixed slurry to 5-10, reacting the mixed slurry at 20-90° C. for 30-120 min, and then evaporating and drying the mixed slurry to obtain phosphate waste residue; as well as Step (2) The phosphate waste residue is mixed with a molecular sieve, a binder, clay and water to form a slurry, and the slurry is spray-formed and calcined to obtain a catalytic cracking catalyst containing the phosphate waste residue.
10. The method according to claim 9, wherein: In step (1), the step of mixing the SAPO molecular sieve mother liquor wastewater and the compound containing the modified metal refers to mixing 60-95% of the SAPO molecular sieve mother liquor wastewater with 5-40% of the modified metal compound on a dry basis, based on the dry basis weight obtained after mixing.
11. The method according to claim 9, wherein: In step (2), mixing the phosphate waste residue with molecular sieve, binder, clay and water to form a slurry means that, based on the dry weight of the catalytic cracking catalyst, 1 to 30 wt % of the phosphate waste residue, 10 to 50 wt % of the molecular sieve, 5 to 40 wt % of the binder and 10 to 50 wt % of the clay are mixed in water to form a slurry with a solid content of 10 to 50 wt %.