Polymer, resin composition and production method and application thereof
By introducing electron-donating groups and aromatic ring structures into the polymer, and adding organic Si compounds, the problem of insufficient adhesion between the polyimide resin and the substrate is solved, and a resin with high adhesion and low linear thermal expansion performance is achieved. Film, suitable for semiconductor devices and display devices.
Patent Information
- Application Number
- CN202111178280.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-09
AI Technical Summary
The adhesion between the polyimide resin and the substrate is insufficient, resulting in low linear thermal expansion performance. Existing improved methods such as the use of silane-containing diamine or acid anhydride monomer synthesis still have defects in adhesion and CTE performance.
Design a polymer containing specific groups, introduce electron-donating groups and aromatic ring structures into the polymer macromolecules, and add organic Si compounds to form a resin composition to improve adhesion and resistance to inorganic substrates. thermal performance while reducing the coefficient of linear thermal expansion.
It achieves high adhesion between the polymer and the inorganic substrate, heat resistance ≥320°C, linear thermal expansion coefficient ≤20ppm/°C, and improves the adhesion between the resin film and the substrate.
Smart Images

Figure CN115960350B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymers and high molecular materials, and in particular to a polymer having high adhesion to a substrate, a resin composition and a production method thereof, and application of the formed resin film. Background Art
[0002] Polyimide resin is an engineering resin with excellent performance. It has excellent heat resistance, drug resistance, and insulation. It is widely used in semiconductor, microelectronics, liquid crystal materials, automobiles, aerospace and other industrial fields.
[0003] Generally, polyimide resin is prepared by solution polymerization of aromatic dianhydride (or aromatic tetracarboxylic acid or aromatic tetracarboxylic acid dialkyl ester) and aromatic diamine to prepare polyimide precursor (polyamic acid or polyamic acid ester), followed by thermal imidization or chemical imidization using a catalyst.
[0004] Polyimide can also be used in color filter films in combination with pigments or dyes, which can greatly simplify the processing procedures of color filter films. In microelectronic devices, color filter films are used as dielectric layers for interlayer insulation, and as buffer layers to reduce stress and improve yield. As a protective layer, it can reduce the impact of the environment on the device. The color filter film can also shield a-particles and reduce or eliminate the soft error of the device. Polyimide is also used as a high-temperature adhesive in the semiconductor industry. When producing digital semiconductor materials and MEMS system chips, the polyimide layer has good mechanical ductility and tensile strength, which helps to improve the adhesion between the polyimide layer and the metal layer deposited on it. At the same time, the high temperature and chemical stability of polyimide also play a role in isolating the metal layer from various external environments.
[0005] The four major applications of polyimide films in the semiconductor and microelectronics industries are:
[0006] (1) Particle shielding film: As the density and chip size of integrated circuits increase, their radiation resistance becomes increasingly important. High-purity polyimide film is an effective radiation and particle shielding material. The reduction film used in the component housing can prevent memory errors caused by the release of radiation from trace amounts of uranium and molybdenum. Of course, the uranium content in the polyimide coating resin must also be very low. The resin for 256kDRAM requires a uranium content of less than 0.1ppb. The excellent mechanical properties of polyimide can also prevent the chip from cracking during the subsequent packaging process.
[0007] (2) Passivation layer and buffer protection layer: In the microelectronics industry, polyimide is widely used as a passivation layer and buffer protection layer. Polyimide coating can effectively prevent electron migration and corrosion. Components protected by polyimide layer have very low leakage current, which can increase the mechanical properties of the device and prevent chemical corrosion. It can also effectively increase the moisture resistance of the components and protect the components. Polyimide film has a buffering effect, which can effectively reduce circuit failures, circuit collapse and open circuits caused by thermal stress, and reduce damage to the device during subsequent processing, packaging, post-processing and use. Polyimide coating can effectively prevent the cracking of plastic packaged devices, and its effect is closely related to the performance of the polyimide material used. Polyimide with good adhesion, glass transition temperature higher than welding temperature, and low water absorption is an ideal inner coating material to prevent device cracking.
[0008] (3) Dielectric materials between layers of multilayer metal interconnect circuits: In multilayer wiring technology, polyimide (mainly PI film) can be used as the dielectric material of multilayer metal interconnect structures. Multilayer wiring technology is a key technology for the development and production of ultra-large-scale, high-density, high-speed integrated circuits. The multilayer metal interconnect on the chip can significantly reduce the interconnection density between devices, reduce the RC time constant and chip area, and greatly improve the speed, integration and reliability of integrated circuits. The multilayer metal interconnect process is different from the commonly used aluminum-based metal interconnect and oxide dielectric insulation process. It mainly uses high-performance polyimide film materials as the insulating layer, copper or aluminum as the interconnect line, and copper chemical mechanical polishing, which mainly utilizes the low dielectric constant, flatness and good mapping performance of polyimide materials.
[0009] (4) Substrate of optoelectronic printed circuit boards: Optical interconnection has the advantages of high bandwidth, high density, and no electromagnetic interference (EMI), and is gradually replacing electrical interconnection for interconnection within the system. Optical interconnection technology is an effective way to solve the bottleneck of electrical interconnection of PCB boards. As one of the most promising PCB products in the future, optoelectronic printed circuit boards (EOPCBs) have expanded from existing electrical connection technology to the following aspects: Add a layer of fluorinated polyimide film light guide layer to the developed PCB, so that the use of circuit boards is extended from the current electrical connection to the field of optical transmission. The refractive index of polyimide can be adjusted by adjusting the fluorine content of the copolymer. The higher the fluorine content, the smaller the refractive index of the fluorinated polyimide film. At present, this polyimide film has been developed in Europe, the United States and Japan, and some of them have begun to be used in small-scale production of optoelectronic printed circuit boards.
[0010] However, the current problem with polyimide is that it does not adhere well to the substrate and has a poor adhesion rate. One way is to use silane-containing diamine or anhydride monomers for synthesis, such as the polyimide disclosed in CN104194618B, and another way is to use silicon-containing substances as additives, such as the photosensitive resins disclosed in CN111830786A and CN109642162A, but the linear thermal expansion properties of the resulting resin films are relatively low. CN112876680A uses a block structure and an imidazole-containing diamine structure to improve adhesion to the substrate, but the adhesion effect is still defective, and similarly, the CTE performance is also poor. Summary of the invention
[0011] In order to improve the adhesion of polyimide to the coated substrate, the present application provides a new polymer, which is prepared into a resin composition to form a resin film, which can not only obtain good adhesion to the substrate but also reduce the linear thermal expansion coefficient.
[0012] The first aspect of the present application is to provide a polymer, especially a polymer having high adhesion to a coated substrate, wherein the substrate is preferably an inorganic plate, especially a silicon plate, a glass substrate, etc.
[0013] The polymer described in the present application preferably contains the following groups represented by formula (II) and / or formula (III):
[0014] -R4'-R1' (III)
[0015] Wherein, in formula (II), R1, R2, and R3 are independently selected from H or a C1-C10 organic group, and at least one of R1, R2, and R3 contains an electron-donating group; R4 is a single bond or a C1-C10 organic group; in formula (III), R1' is a C1-C10 organic group and also contains an electron-donating group; R4' is a single bond or a C1-C10 organic group.
[0016] In a preferred embodiment, the electron donating group can be any one or more of -NR5R6, -O-R5, -S-R5, -O-R7-NR5R6, -NR6-R7-O-R5; wherein R5 and R6 are independently selected from H and C1-C9 alkyl; R7 is preferably a single bond or C1-C9 alkylene.
[0017] Specifically, the C1-C9 alkyl group may be preferably a C1-C6 alkyl group, more preferably a C1-C4 alkyl group, examples of which include: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl.
[0018] Specifically, the C1-C9 alkylene group may be preferably a C1-C6 alkylene group, more preferably a C1-C4 alkylene group, examples of which include: -CH2-, -CH2-CH2-, -CH(CH3)-CH2-, -CH2-CH2-CH2-, -CH(CH3)-CH2-CH2-, -CH2-CH(CH3)-CH2-, -CH2-CH(CH3)-CH2-, -CH2-CH2-CH2-CH2-.
[0019] In a preferred embodiment, the electron donating group may be selected from:
[0020] -OH, -CH2-OH, -CH2-CH2-OH, -CH2-CH2-CH2-OH, -CH(CH3)-OH, -CH2-CH(CH3)-OH, -CH(CH3)-CH2-OH, -CH2-CH(C H3)-CH2-OH, -O-CH3, -O-CH2-CH3, -O-CH(CH3)-CH3, -NH2, -NH-CH3, -NH-CH2-CH3, -NH-CH(CH3)-CH3, -N(CH3)2 , -N(CH3)(CH2-CH3), -N(CH2-CH3)2, -NH-CH(CH3)-CH3, -O-NH-CH3, -ON(CH3)2, -O-CH2-NH-CH3, -NH-O-CH3, -NH-O-CH2-CH3, -NH-O-CH(CH3)2, -NH-CH2-O-CH3, -NH-CH2-O-CH2-CH3, -N(CH3)-CH2-O-CH3, -SO2-OH, one or more thereof.
[0021] In a preferred embodiment, the groups represented by formula (II) and / or formula (III) may be present in any one or more of the side chains (branches) and terminal groups of the polymer.
[0022] In a preferred embodiment, in the groups represented by formula (II) and / or formula (III) located in the side chain of the polymer, the C1-C10 organic group is preferably a saturated organic group, especially a chain organic group, and more preferably an organic group with less steric hindrance, for example, it may not contain tertiary carbon atoms.
[0023] Specifically, the group represented by formula (II) and / or formula (III), when R4 and R4' are single bonds, can be selected from:
[0024]
[0025] Aromatic ring bonding of the polymer backbone.
[0026] In a preferred embodiment, in the groups represented by formula (II) and / or formula (III) at the terminal groups of the polymer, R4 and R4' are preferably organic groups containing aromatic rings, and the aromatic rings may be aromatic hydrocarbon rings or aromatic rings containing heteroatoms.
[0027] Specifically, R4 and R4' can be selected from:
[0028] Any one or more of .
[0029] In a preferred embodiment, the C1-C10 organic group may contain heteroatoms, such as any one or more of N, O, S, and P.
[0030] In a preferred embodiment, the polymer is any one or more of polyimide and polyimide precursor.
[0031] In a preferred embodiment, the polymer has a polyimide structural unit shown in the following formula (I):
[0032]
[0033] Wherein, X, X", Y, and Y" are independently aromatic rings, such as aromatic hydrocarbons or heteroaromatic rings, and may be monocyclic, bicyclic, or multicyclic structures, such as benzene rings, biphenyls, and condensed ring structures. Specific preferred aromatic rings may be selected from:
[0034]
[0035] Any one or more of; R5, R5' are independently selected from H or an organic group containing C1~10.
[0036] In a preferred embodiment, the group represented by formula (II) and / or formula (III) located on the side chain of the polymer is linked to the aromatic ring of the polymer.
[0037] The second aspect of the present application is to provide a resin composition, which includes the polymer mentioned in the present application. When made into a resin film, it has high adhesion to the coated substrate, wherein the substrate is preferably an inorganic plate, especially a silicon plate, a glass substrate, etc.
[0038] The present application provides a resin composition, comprising the polymer provided in the present application; preferably, in the resin composition, with the molar ratio of all polymer repeating units contained therein being 100 mol%, the total molar content of the groups represented by formula (II) and formula (III) is preferably 1 to 80 mol%, preferably 5 to 70 mol%, and more preferably 10 to 62 mol%; wherein, it is particularly noted that the polymer may contain formula (II), may contain formula (III), or may contain formula (II) and formula (III).
[0039] In a preferred embodiment, the resin composition further contains units or side chains of Si-containing organic compounds, and preferably the units or side chains are polymerized into the polymer by a Si-containing compound with a reactive group in a polymerization reaction, or are linked to the polymer by a reaction between the Si-containing compound with a reactive group and a polymer side group.
[0040] In a preferred embodiment, in the resin composition, taking the molar ratio of all polymer repeating units as 100 mol%, the ratio of the units or side chains of the Si-containing organic compound is 0.1 to 20 mol%, preferably 0.5 to 15 mol%, and more preferably 1 to 10 mol%.
[0041] The third aspect of the present application is to provide a method for preparing the polymer of the present application, comprising:
[0042] The polymerizable monomers are subjected to a polymerization reaction, wherein some of the polymerizable monomers contain groups represented by formula (II) and / or formula (III), or after the polymerization reaction, the polymer is capped with a compound containing groups represented by formula (II) and / or formula (III), so that the polymer ends have groups represented by formula (II) and / or formula (III).
[0043] In a preferred embodiment, the polymerization is addition polymerization or condensation polymerization.
[0044] In a preferred embodiment, the polymerizable monomers are diamine monomers and dianhydride (or tetracarboxylic acid corresponding to the dianhydride) monomers, wherein part of the diamine monomers and / or part of the dianhydride monomers contain groups represented by formula (II) and / or formula (III).
[0045] More preferably, the molar ratio of the diamine monomer to the dianhydride monomer is preferably 40:60 to 60:40, more preferably 43:57 to 57:43, and more preferably 45:55 to 55:45.
[0046] In a preferred embodiment, the diamine monomer is HN2-Y-NH2.
[0047] In a preferred embodiment, the dianhydride monomer is
[0048] In a preferred embodiment, in the preparation method, at least part of the polymerizable monomers are Si-containing organic compounds.
[0049] In a preferred embodiment, the preparation method further comprises: after the polymerization reaction is completed, the polymer side group reacts with the organic compound containing Si to form a side chain of the organic compound containing Si.
[0050] The third aspect of the present application is to provide a resin film, which contains the polymer of the present application; or is prepared from the resin composition of the present application.
[0051] The fourth aspect of the present application is to provide an application of the resin composition, preferably applied to display devices or products, semiconductor components or products. In particular, the polymer is bonded to inorganic plates, especially silicon plates, glass substrates, etc.
[0052] Beneficial effects of the present invention:
[0053] (1) By introducing electron-donating groups into polymer macromolecules, the chemical electron supply balance between polymer materials and inorganic materials is increased, thereby increasing the adhesion between them.
[0054] (2) Design the polymer macromolecular structure and introduce an aromatic ring structure with good heat resistance to improve its heat resistance to ≥320°C; the proportion of the aromatic ring can be determined by the polymerization raw materials and ratio.
[0055] (3) Design the polymer macromolecular structure and introduce rigid single benzene ring, biphenyl, condensed ring and other structures to reduce the linear thermal expansion coefficient (CTE) to ≤20ppm / ℃.
[0056] (4) In order to further improve the adhesion between the resin film and the inorganic substrate, a small amount of organic Si-based compounds is added. The organic Si-based compounds have a certain flexibility, and while not losing the CTE effect, the adhesion between the provided resin film and the substrate is further improved. DETAILED DESCRIPTION
[0057] The present application provides a polymer, taking polyimide as an example, which has a structural unit shown in formula (I-1) and / or formula (I-2), and the side chain or end of the polymer contains a group shown in formula (II) and / or formula (III):
[0058]
[0059] -R4'-R1' (III)
[0060] The group represented by formula (II) and / or formula (III) may be located on the diamine monomer of the synthetic polymer and / or on the dianhydride monomer of the synthetic polymer, for example:
[0061] Wherein, m and n are independently integers, m and m' represent the number of groups represented by formula (II) and / or formula (III) in the diamine monomer, n and n' represent the number of groups represented by formula (II) and / or formula (III) in the dianhydride monomer, X' replaces the groups represented by formula (II) and / or formula (III) to form X and X' groups, and Y' replaces the groups represented by formula (II) and / or formula (III) to form Y and Y' groups. The above-mentioned diamine monomer and dianhydride monomer are polymerized to form a polymer having groups represented by formula (II) and / or formula (III) in the side chain.
[0062] During the polymer reaction, the molar ratio of diamine to dianhydride is preferably 40:60 to 60:40, more preferably 43:57 to 57:43, and more preferably 45:55 to 55:45.
[0063] Preferably, in the structural formula (I-1) and / or the formula (I-2), X, X", Y, Y" (raw materials are dianhydride and diamine) all contain aromatic rings with thermal stability. In the preparation method, raw materials containing benzene rings are used, and the content of benzene rings with high heat resistance accounts for a large proportion, so that the matrix polyimide polymer has excellent thermal stability; in addition, among the raw materials containing benzene rings used, monophenyl, biphenyl, and condensed ring raw materials account for a larger proportion, so as to obtain the rigidity of the polymer macromolecular chain and reduce the linear thermal expansion coefficient. Specifically, the aromatic rings of X, X", Y, Y" can be selected from:
[0064]
[0065] Any one or more of .
[0066] In addition, the present application can also form a group represented by formula (II) and / or formula (III) at the end of the polymer, which can be achieved by using a capping agent with a group represented by formula (II) and / or formula (III).
[0067] In formula (II) and / or formula (III), R1', R1, R2, and R3 are independently organic groups containing H atoms (R1' is not H) or 0 to 10 C atoms, and at least one of R1', R1, R2, and R3 contains an electron-donating group; wherein the electron-donating group is preferably: dialkylamino, alkylamino, amino (-NH2), hydroxyl (-OH), alkoxy, and more preferably contains OH or an organic group with less steric hindrance.
[0068] R4 and R4' represent 0 to 10 carbon atoms and may contain other heteroatoms (S, O, P, N).
[0069] Examples of the structures represented by formula (II) and / or formula (III) as side chains include:
[0070] Preferably, the capping agent is exemplified as follows:
[0071]
[0072]
[0073]
[0074]
[0075] The present application provides a resin composition, comprising a polymer provided by the present application. The resin composition may also include other polymers, preferably one or more combinations of polyimide, polyamic acid, and polyamic acid ester. Wherein, the molar content of the structure of formula (II) and formula (III) relative to the repeating unit (100mol%) of the polymer structure is: 1 to 80mol%, preferably 5 to 70mol%, and more preferably 10 to 62mol%. For example, for every 100 repeating units in the polymer, the sum of the number of units shown in formula (II) and formula (III) is 1-80, preferably 5-70, and more preferably 10-62. The purpose of adding the structure of formula (II) and / or formula (III) is to improve the adhesion between the polymer resin film and the inorganic plate (silicon plate, glass substrate, etc.). The resin composition may also contain units of Si-based organic compounds, and more preferably, the Si-based organic compounds contain reactive functional groups, which are polymerized into the polymer in a polymerization reaction; preferably, the molar content of the units of the Si-based organic compounds relative to the repeating units (100 mol%) of the polymer is 0.1 to 20 mol%, preferably 0.5 to 15 mol%, and more preferably 1 to 10 mol%. For example, for every 100 repeating units of the polymer structure, the number of units of the Si-based organic compound is 0.1-20, preferably 0.5-15, and more preferably 1-10. The purpose of adding Si-based organic compounds is to further improve the adhesion between the polyimide resin film and the inorganic plate (silicon plate, glass substrate, metal plate, ceramic plate, etc.). Si-based organic compounds have a certain flexibility, and if too much is added, the CTE will increase, and the decomposition temperature of the polymer will decrease.
[0076] In a preferred embodiment, the resin composition may further include a solvent. After the slurry is made by containing a solvent, the coating performance can be improved. In particular, preferably γ-butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether and diethylene glycol, monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl Butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol ether, ethylene glycol monoethyl ether, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether ethyl ester, propylene glycol monoethyl ether acetate, ethyl lactate and other esters, 2-hydroxy-2- any one or more of ethyl methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl glycolate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propyl valerate, ethyl butyrate, n-propyl butyrate, isobutyric acid butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate, aromatic compounds such as toluene, xylene, amides, and solvents such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0077] The amount of the solvent used is preferably 55-98% by weight of the resin composition.
[0078] In a preferred embodiment, the viscosity of the resin composition is preferably 0.1 cP to 20000 cP.
[0079] Other additives may be added to the resin composition according to functional requirements. For example, in order to make the CTF effect of the polymer better, a cross-linking agent can be added; preferably, the cross-linking agent is a thermal cross-linking agent, more preferably a hydroxymethyl compound, a methoxymethyl compound, a urea compound, an epoxy compound, an oxetane compound, etc. Specifically, the available thermal cross-linking agents include ML-236TMP, 4-Methylol 3M6C, ML-MC, ML-TBC, 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, TriML-P, TriML-35XL, TriML-TrisCR-HAP, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP; preferably, the cross-linking agent accounts for 0.5-50% by weight of the resin composition, and more preferably 3-40% by weight. For example, inorganic particles are used to enhance the heat resistance of the resin film after heat treatment and to impart high elasticity to the film. Preferred inorganic particles include, but are not limited to, silica, titania, alumina, and zirconia.
[0080] Preparation method of polymer:
[0081] The monomers of the polymer are subjected to polymerization reaction, wherein some of the polymerized monomers contain groups represented by formula (II) and / or formula (III), or after the polymerization reaction, the polymer is capped with a compound containing groups represented by formula (II) and / or formula (III), and the polymer ends are provided with groups represented by formula (II) and / or (III); preferably, the molar ratio of the diamine monomer to the dianhydride monomer is preferably 40:60 to 60:40, more preferably 43:57 to 57:43, and more preferably 45:55 to 55:45; preferably, the weight average molecular weight of the polymer is in the range of 8000 to 800000, further preferably 12000 to 500000, and more preferably 15000 to 250000. The weight average molecular weight of the polymer can be tested by gel permeation chromatography (GPC, Shimadzu LC-20AD).
[0082] Preferably, the diamine monomer is HN2-Y-NH2; the dianhydride monomer is More specifically, the diamine monomers containing formula (II) and / or formula (III) can be listed as follows:
[0083]
[0084]
[0085] The dianhydride monomers containing formula (II) and / or formula (III) can be listed as follows:
[0086]
[0087] Preparation method of resin composition:
[0088] (1) The polymer provided in the present application is placed in a glass flask or a stainless steel container, and a solvent and / or other required polymers and additives are added as needed; (2) The resin composition involved in the present application is obtained by mixing by dissolving using a mechanical stirrer, ultrasonic waves, a stirring degassing machine, etc.
[0089] The resin composition provided in the present application may only contain the polymer provided in the present application; or it may be obtained by mixing the polymer provided in the present application with other types of polymers. Finally, the molar content of the structure of formula (II) and formula (III) relative to the repeating unit (100 mol%) of the polymer structure is 1 to 80 mol%, preferably 5 to 70 mol%, and more preferably 10 to 62 mol%. For example, for every 100 repeating units in the polymer, the sum of the number of units represented by formula (II) and formula (III) is 1 to 80, preferably 5 to 70, and more preferably 10 to 62.
[0090] The viscosity of the resin composition involved in the present application is preferably 0.1cP to 20000cP; when the viscosity is above 0.1cP and below 20,000cP, by adjusting the appropriate solid content, a resin film of target thickness can be obtained, the uniformity of film performance can be controlled, and good coating efficiency can be obtained. The viscosity test can be performed using an E-type viscometer. In addition, in order to remove foreign matter in the resin composition, the resin composition can be filtered with a filter with a pore size of 0.01-5μm. The materials used as the main filter components in the filter include polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc.; when the resin composition contains fluorine-based surfactants and / or surface modifiers, polyethylene (PE) is preferably used as the material of the main filter components in the filter.
[0091] The viscosity of the resin composition can be measured by using an E-type viscometer (BROOKFIELD DV2T RV) with the temperature controlled at 25°C ± 0.1°C and a suitable measuring range.
[0092] <Method for preparing resin film>
[0093] The resin film involved in the present application can be prepared by the following method: coating the resin composition involved in the present application on a substrate, and then performing drying, heat treatment and curing processes to obtain the resin film, which can also be called a cured film.
[0094] The substrate may be made of silicon wafer, ceramics, gallium arsenide, metal, glass, metal oxide insulating film, silicon nitride, ITO, IZO, amorphous silicon, microcrystalline silicon, polycrystalline silicon, IGZO, etc., but is not limited to these.
[0095] The coating method may be one of spin coating, spray coating, slit coating, inkjet coating and / or a combination of multiple methods; in terms of the uniformity of the thickness of the resulting resin film, it is preferred to use a coating method that uses slit coating, a combination of slit coating and spin coating, etc.
[0096] The drying method may be one of oven, heating plate, infrared ray and / or a combination of multiple methods; in terms of production stability, the drying conditions are preferably a drying temperature in the range of 50°C to 150°C and a drying time in the range of 2 minutes to 3 hours; in terms of film stability, the drying temperature is preferably 80°C to 130°C. In addition, the drying method may be a drying method that is carried out in one stage, two stages or more stages.
[0097] The heat treatment curing method may use one of an oven, a heating plate, infrared rays and / or a combination of multiple methods; from the perspective of production stability, the heat treatment conditions preferably have a heat treatment temperature in the range of 150°C to 500°C as the curing temperature, and a heat treatment time in the range of 2 minutes to 5 hours. In addition, the heat treatment method may be a heat treatment method that is carried out in one stage, two stages or more stages; from the perspective of warping of the resin film, a heat treatment method that is carried out in multiple stages is preferred.
[0098] The resin film involved in the present application can be applied to electronic components such as semiconductor devices and multilayer wiring boards; specifically, it can be suitably applied to passivation films in semiconductor devices, surface protection films of semiconductor elements, interlayer insulating layers, interlayer insulating films of multilayer wiring for high-density installation, substrates of organic light-emitting elements, insulating layers, planar layers of thin-film transistors, interlayer insulating films of thin-film transistors, etc.; in addition, when the resin composition contains conductive fillers, it can also be used as a wiring material, but various structures can be adopted and are not limited to this.
[0099] The polymer provided in this application is used to prepare the resin composition required by this application, and after being prepared into the resin film provided in this application, the adhesion to the inorganic plate (such as silicon plate, glass substrate, etc.) is ≥0.2N / cm, the heat resistance is ≥320℃, and the linear thermal expansion coefficient (CTE) is ≤20ppm / ℃. It can be well bonded to inorganic plates such as silicon plate, glass substrate, etc., and used to make display or semiconductor devices or products.
[0100] The following specific examples are used to illustrate the content of this application. The compounds used in the following examples are as follows:
[0101] Compound 1: 1,2,4,5-pyromellitic dianhydride (PMDA) (Cas No.: 89-32-7)
[0102]
[0103] Compound 2: 3,3,4,4-biphenyltetracarboxylic acid (BPDA) (Cas No.: 2420-87-3)
[0104]
[0105] Compound 5: p-phenylenediamine (PDA) (Cas No.: 106-50-3)
[0106]
[0107] Compound 6: 3,3'-Diaminodiphenyl sulfone (Cas No.: 599-61-1)
[0108]
[0109] Compound 7: (4,4'-diamino-[1,1'-biphenyl]-3-yl), methanol can be obtained by ordinary SUZUKICOUPLING (coupling reaction);
[0110]
[0111] For example, 4-aminophenylboronic acid pinacol ester (Cas No.: 214360-73-3) and 2-amino-5-bromobenzyl alcohol (Cas No.: 226713-43-5) can react in the presence of a palladium catalyst and a base to generate compound 7.
[0112] Compound 8: 4-amino-N-(4'-((1-(4-aminophenyl)-1-(11-oxyalkylene)ethyl)amino)-3,3'-bis(hydroxymethyl)-[1,1'-biphenyl]-4-yl)benzamide, can be obtained by a common coupling reaction;
[0113]
[0114] For example, 2-amino-5-bromobenzyl alcohol (CAS: 226713-43-5) is used to obtain compound 8-1 under ZnCl2 catalysis: Then compound 8-1 is reacted with p-nitrobenzoyl chloride under organic base conditions to obtain compound 8-2:
[0115]
[0116] Finally, compound 8-2 is reduced to generate compound 8.
[0117] Compound 9: 1,1,3,3-Tetramethyl-1,3-bis(3-aminopropyl)disiloxane (CAS No.: 2469-55-8)
[0118]
[0119] Compound 10: Bi-terminal aminosiloxane (manufactured by Dongguan Sanchuan Chemical Technology Co., Ltd., molecular weight about 300)
[0120] Compound 11: 2-amino-5,7-naphthalene disulfonic acid; 2-naphthylamine-5,7-disulfonic acid (Cas No.: 118-33-2)
[0121]
[0122] Compound 12: 4-sulfophthalic anhydride (Cas No.: 134-08-7)
[0123]
[0124] Compound 13: 3,4'-diaminodiphenyl ether (Cas No.: 2657-87-6)
[0125]
[0126] Compound 14: 4,4'-oxydiphthalic anhydride (Cas No.: 1823-59-2)
[0127]
[0128] Compound 15: 4-ethynylaniline (Cas No.: 14235-81-5)
[0129]
[0130] Example 1
[0131] Under nitrogen atmosphere, compound 1 (10.3 g, 0.047 mol) and compound 6 (11.2 g, 0.045 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; compound 11 (0.7 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 1.
[0132] Example 2
[0133] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol) and compound 5 (4.9 g, 0.045 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; compound 11 (0.7 g, 0.002 mol) was added, and the reaction was continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 2.
[0134] Example 3
[0135] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol), compound 5 (4.8 g, 0.044 mol) and compound 9 (0.3 g, 0.001 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; compound 11 (0.7 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 3.
[0136] Example 4
[0137] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol), compound 5 (4.8 g, 0.044 mol) and compound 10 (0.4 g, 0.001 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; compound 11 (0.7 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 4.
[0138] Example 5
[0139] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol), compound 5 (4.2 g, 0.039 mol), compound 9 (0.3 g, 0.001 mol) and compound 13 (1.0 g, 0.005 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; then compound 11 (0.7 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 5.
[0140] Example 6
[0141] Under nitrogen atmosphere, compound 1 (10.3 g, 0.047 mol) and compound 6 (11.2 g, 0.045 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; compound 12 (0.5 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 6.
[0142] Example 7
[0143] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol), compound 5 (2.2 g, 0.020 mol), compound 7 (4.0 g, 0.019 mol), compound 9 (0.3 g, 0.001 mol) and compound 13 (1.0 g, 0.005 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 h; then compound 11 (0.7 g, 0.002 mol) was added, and the stirring reaction continued at 65°C for 2 h. Then 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 h to obtain resin 7.
[0144] Example 8
[0145] Under nitrogen atmosphere, compound 2 (13.8 g, 0.047 mol), compound 5 (2.5 g, 0.023 mol), compound 8 (9.3 g, 0.019 mol) and compound 13 (1.0 g, 0.005 mol) were added to the reactor and dissolved in 120 ml of NMP, and stirred at 65°C for 4 hours. Then, 13.2 g (0.09 mol) of N,N-dimethylformamide diethyl acetal was added, and the reaction was carried out at 40°C for 1 hour; 30 g of acetic acid was added at below 30°C, and after stirring for 1 hour, it was added to 2 L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 hours to obtain resin 8.
[0146] Resins 1 to 8 described in Examples 1 to 8 were dissolved in γ-butyrolactone to prepare resin compositions with a resin concentration of 18%, thereby obtaining resin compositions 1 to 8 of Examples 9 to 16. The viscosity of the resin compositions was tested to be in the range of 3000 to 8000 cP.
[0147] Embodiment 17
[0148] 15.0 g of resin 1 obtained in Example 1 and resin 7 obtained in Example 7 were weighed respectively and added to 137 g of γ-butyrolactone to prepare a resin composition with a resin concentration of 18%, thereby obtaining resin composition 9. The viscosity was tested to be 5013 cP.
[0149] Embodiment 18
[0150] The same method as in Example 1 was used except that Compound 11 was replaced by Compound 15. Resin A was obtained. Then 15 g of Resin A and 15 g of Resin 8 obtained in Example 8 were weighed and added to 137 g of γ-butyrolactone to prepare a resin composition having a resin concentration of 18%, thereby obtaining Resin Composition 10. The viscosity was tested to be 6013 cP.
[0151] Comparative Example 1
[0152] The same method as in Example 1 was used except that Compound 11 was replaced by Compound 15. Resin A was obtained. Then 30 g of Resin A was weighed and added to 137 g of γ-butyrolactone to prepare a resin composition having a resin concentration of 18%, thereby obtaining Resin Composition A. The viscosity was tested to be 5413 cP.
[0153] Comparative Example 2
[0154] The same method as in Example 5 was used except that compound 11 was replaced by compound 15. Resin B was obtained. Then 30 g of resin B was weighed and added to 137 g of γ-butyrolactone to prepare a resin composition with a resin concentration of 18%, thereby obtaining resin composition B. The viscosity was tested to be 3993 cP.
[0155] The compounds used in Examples 1 to 8 and Comparative Examples 1 to 2 are detailed in Table 1-1 and Table 1-2.
[0156] The resin compositions obtained in Examples 9 to 16 and Comparative Examples 3 to 4 were tested for coating performance, adhesion, heat resistance, and linear thermal expansion coefficient (CTE) as described in the present application, and the results are shown in Table 2.
[0157] Table 1-1 Compounds
[0158]
[0159] Table 1-2 Compounds
[0160]
[0161]
[0162] Table 2
[0163]
[0164]
[0165] 2. Polymer performance test method:
[0166] (1) Sample preparation
[0167] The solution of the resin composition was spin-coated on an 8-inch silicon wafer, and then baked on a heating plate at 120°C for 3 minutes to obtain a pre-baked film. The pre-baked film was then baked using an inert gas oven (apparatus CLH-21CD(V)-CCC manufactured by Koyo Thermo Systems Co., Ltd.), and the oxygen concentration was set to less than 20 ppm. The temperature was raised to 250°C at a rate of 5°C / min, and heat-treated at 250°C for 20 minutes, and then raised to 350°C at a rate of 10°C / min, and heat-treated at 350°C for 60 minutes, and then cooled to 50°C at a rate of 5°C / min to obtain a baked film. The film thickness was tested using a step profiler (KLA Tencor P-7), and the coating process was adjusted to obtain a film thickness of about 10±0.5μm at the center point of the baked film.
[0168] (2) Heat resistance test
[0169] The baked film obtained by the above (1) is peeled off and 10 mg is taken out, and placed in TGA (TA Q50), the test atmosphere is nitrogen, the heating rate is 20°C / min, and the temperature T when the weight loss is 1% is tested. When the temperature is 400°C≦T, the heat resistance is excellent, represented by A; when the temperature is 350°C≦T<400°C, the heat resistance is excellent, represented by B; when the temperature is 320°C≦T<350°C, the heat resistance is good, represented by C; when the temperature is T<320°C, the heat resistance is poor, represented by D.
[0170] (3) Adhesion peeling test between cured film (imidized resin film) and substrate
[0171] The baked film obtained in the above (1) was subjected to a 90° peel test using a universal testing machine (RTG1210) to obtain a peel force S. When the peel force is 0.4 N / cm≦S, the adhesion is excellent, indicated by A; when the peel force is 0.3 N / cm≦S<0.4 N / cm, the adhesion is good, indicated by B; when the peel force is 0.2 N / cm≦S<0.3 N / cm, the adhesion is good, indicated by C; when the peel force S<0.2 N / cm, the adhesion is poor, indicated by D.
[0172] (4) Evaluation of coating performance
[0173] The baked film obtained in (1) above is used to measure the film thickness in four directions (perpendicular to each other) with the center point of the baked film as the base point. The film thickness is measured at 10 points in each direction, and then the standard deviation δ of the film thickness at 40 points is calculated. When the standard deviation δ of the film thickness is ≤ 0.10, the coating performance is evaluated as excellent, represented by A; when the standard deviation 0.10 < δ < 0.15, the coating performance is evaluated as good, represented by B; when the standard deviation 0.15 < δ < 0.20, the coating performance is evaluated as good, represented by C; when the standard deviation 0.20 < δ, the coating performance is evaluated as poor, represented by D.
[0174] (5) Linear thermal expansion coefficient (CTE) test
[0175] The baked film obtained by the above (1) is peeled off and cut into the required size, and placed in an instrument (TMA4000 manufactured by PerkinElmer) for testing. The atmosphere is nitrogen and the heating rate is 10°C / min. The linear thermal expansion coefficient CTE of 50-200°C is measured. When the linear thermal expansion coefficient CTE is ≤10, the performance is excellent, represented by A. When the linear thermal expansion coefficient is 10<CTE≤15, the performance is good, represented by B. When the linear thermal expansion coefficient is 15<CTE≤20, the performance is good, represented by C. When the linear thermal expansion coefficient is 20<CTE, the performance is poor, represented by D.
[0176] The specific embodiments of the application are described in detail above, but they are only examples, and the application is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the application are also within the scope of the application. Therefore, the equivalent changes and modifications made without departing from the spirit and scope of the application should be included in the scope of the application.
Claims
1. A polymer, characterized in that The monomers are composed of compound 2, compound 5, compound 7, compound 13, compound 9 and compound 11, and the molar ratio of compound 2, compound 5, compound 7, compound 13, compound 9 and compound 11 is 47:20:19:5:1:2; Or it is composed of compound 2, compound 5, compound 8 and compound 13, wherein the molar ratio of compound 2, compound 5, compound 8 and compound 13 is 47:23:19:5; in, The structure of compound 2 is: , The structure of compound 5 is: , The structure of compound 7 is: , The structure of compound 8 is: 、 The structure of compound 13 is: , The structure of compound 9 is: , The structure of compound 11 is: .
2. A resin composition, characterized in that The invention comprises the polymer according to claim 1.
3. A resin film prepared from the resin composition according to claim 2.
4. The resin film according to claim 3, characterized in that The resin film is bonded to the inorganic plate.
5. The resin film according to claim 4, characterized in that The inorganic plate includes a silicon plate or a glass substrate.
6. An application of the resin composition according to claim 2, characterized in that: Applicable to display devices or semiconductor components.