A method for preparing high-purity metallic bismuth

By reacting bismuth-containing raw materials with phosphate impurity removers and oxidants under an inert atmosphere to generate phosphate scum to remove impurities, the existing technology problems of high investment in high-purity metal bismuth production equipment and low impurity removal efficiency are solved, and the The efficient preparation of high-purity metal bismuth meets the impurity limit requirements of the cosmetics industry.

CN115961152BActive Publication Date: 2024-10-29CENT SOUTH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211534873.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-10-29
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The existing vacuum distillation method and regional smelting method have problems such as high equipment investment, complex operation, and low impurity removal efficiency when producing high-purity bismuth metal. It is difficult to meet the needs of the pharmaceutical and cosmetics industry for heavy metal impurity limits.

Method used

The bismuth-containing raw material is melted under an inert atmosphere and reacts with a phosphate impurity remover and oxidant to generate phosphate scum to remove negative potential impurities, thereby achieving the preparation of high-purity metallic bismuth.

Benefits of technology

It has achieved a short process flow, low equipment investment, and high impurity removal efficiency. The content of negative potential impurities such as zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt in the product reaches the Bi99.999 standard, which meets the requirements of the cosmetics industry. Safety technical specification requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of non-ferrous metal metallurgy. The present invention provides a method for preparing high-purity metallic bismuth, comprising the following steps: melting a bismuth-containing raw material under an inert atmosphere to obtain a molten bismuth liquid; adding a phosphate impurity remover and an oxidant to the molten bismuth liquid for reaction under an inert atmosphere, and the negative potential impurities in the molten bismuth liquid generate phosphate scum, and the high-purity metallic bismuth can be obtained by removing the phosphate scum. The present invention can achieve deep removal of negative potential impurities such as lead, zinc, arsenic, iron, nickel, cadmium, chromium, tin, magnesium, and cobalt in crude bismuth to obtain high-purity metallic bismuth. Compared with traditional crude bismuth impurity removal and purification processes such as vacuum distillation and zone smelting, this method has a short process flow, low equipment investment, easy industrial operation, high impurity removal efficiency, and good product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nonferrous metal metallurgy, and in particular to a method for preparing high-purity metallic bismuth. Background Art

[0002] Bismuth metal has unique physical and chemical properties and can be used as a metallurgical additive to improve the metal's processing properties and wear resistance. It can be used to prepare bismuth-based low-melting-point fusible alloys. High-purity bismuth can be used as a heat carrier or coolant in nuclear reactors and in thermocouples. Bismuth-containing raw materials typically contain impurities such as lead, copper, silver, tin, and arsenic, requiring crude refining and refining to increase the purity of the metal. Crude bismuth can be purified through two methods: pyrorefining and electrorefining. Electrorefining can remove impurities such as gold, silver, lead, iron, tin, and tellurium. However, electrorefining requires large fixed investments in plant and equipment, a long refining cycle, and a preliminary pyrorefining process to remove impurities such as arsenic, antimony, and copper, which can significantly affect the electrorefining process. This process is complicated and has been gradually replaced by pyrorefining. Fire refining of crude bismuth is typically carried out in steel refining kettles. It typically undergoes a series of steps, including smelting, sulfur removal for copper removal, oxidation for arsenic and antimony removal, alkaline refining for tellurium and tin removal, zinc removal for silver removal, chlorination for lead and zinc removal, and final refining, to produce refined bismuth with a purity of 99.99%. With increasing understanding of metallic bismuth, non-toxic, high-purity bismuth is widely used in the pharmaceutical, electronics, metallurgy, chemical, and nuclear industries, resulting in a growing demand for high-purity bismuth. However, the purity of refined bismuth still fails to meet the heavy metal impurity limits required by industries like pharmaceuticals and cosmetics.

[0003] Currently, the main methods for producing high-purity metallic bismuth are vacuum distillation and zone melting. Vacuum distillation involves separating impurities from bismuth through distillation under vacuum conditions. However, due to the similar saturated vapor pressures of bismuth, lead, and antimony, vacuum distillation is less effective in removing impurities like lead and antimony. Furthermore, it places high demands on vacuum equipment operation and process control. Zone melting utilizes the segregation effect. As molten bismuth cools and crystallizes, impurities condense before bismuth and precipitate at the edges of the container. This results in fewer impurities at the center of the bismuth ingot than at the edges. Repeated refining achieves the desired purification goal. However, this method suffers from long operation times and low production efficiency.

[0004] Therefore, in view of the shortcomings and disadvantages of the existing vacuum distillation method and zone melting method for producing high-purity metallic bismuth, a preparation method for high-purity metallic bismuth with low equipment investment, simple and easy operation and high efficiency of impurity element removal has been developed, which has important significance and application value. Summary of the Invention

[0005] The present invention aims to address the shortcomings of existing technologies by providing a method for preparing high-purity metallic bismuth. The method can efficiently remove negatively charged impurity metals from metallic bismuth. It has the advantages of a short process flow, low fixed asset investment, ease of industrial operation, high impurity removal efficiency, and high product quality.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing high-purity metallic bismuth, comprising the following steps:

[0008] (1) melting a bismuth-containing raw material under an inert atmosphere to obtain a molten bismuth liquid;

[0009] (2) A phosphate impurity remover, an oxidant, and a molten bismuth solution are reacted under an inert atmosphere, and negative potential impurities in the molten bismuth solution are converted into phosphate scum, which is removed to obtain high-purity metallic bismuth.

[0010] Preferably, the bismuth-containing raw material in step (1) comprises a mixture of crude metallic bismuth and bismuth oxide or crude metallic bismuth with a bismuth grade of more than 95%.

[0011] Preferably, when the bismuth-containing raw material in step (1) is a mixture of crude metallic bismuth and bismuth oxide, the bismuth-containing raw material is mixed with a reducing agent and then melted; the reducing agent is carbon powder; and the mass ratio of the reducing agent to the bismuth-containing raw material is 1 to 10:100.

[0012] Preferably, the negative potential impurity elements in the bismuth-containing raw material in step (1) include one or more of zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt, wherein the content of zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt is independently 0.0001 to 3%.

[0013] Preferably, the melting temperature in step (1) is 400-1100° C.; and the melting time is 50-200 min.

[0014] Preferably, the phosphate impurity remover in step (2) comprises one or more of bismuth phosphate, ammonium salt of phosphorus oxyacid and ammonium polyphosphate; the bismuth phosphate is BiPO4; the ammonium salt of phosphorus oxyacid is (NH4)3PO4, NH4PO3, (NH4)2HPO4 or NH4H2PO4; the ammonium polyphosphate is (NH4,H)4P2O7, (NH4,H)5P3O 10 、(NH4,H)6P4O 13 , NH4H2PO2 or H 12 N3O3P.

[0015] Preferably, the amount of the phosphate impurity remover in step (2) is 1 to 10 times the theoretical amount.

[0016] Preferably, the oxidant in step (2) comprises one or more of NaNO3, NaNO2, Na2O2, KNO3, KNO2 and K2O2; the amount of the oxidant used is 0.1 to 3 times the theoretical amount.

[0017] Preferably, the reaction temperature in step (2) is 400-1100° C.; and the reaction time is 30-300 min.

[0018] Preferably, the inert atmosphere in step (1) and step (2) is a nitrogen atmosphere and / or an argon atmosphere.

[0019] The beneficial effects of the present invention are:

[0020] (1) Compared with traditional crude bismuth impurity removal and purification processes such as vacuum distillation and zone smelting, the present invention has the advantages of a short process flow, low equipment investment, easy industrial operation, and high impurity removal efficiency;

[0021] (2) The content of negative potential impurities such as zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt in the high-purity metallic bismuth product obtained by the preparation method of the present invention meets the requirements of the Bi99.999 (YS / T818-2012) standard, especially the content of lead, arsenic, and cadmium meets the requirements of the safety technical specifications of the cosmetics industry. DETAILED DESCRIPTION

[0022] The present invention provides a method for preparing high-purity metallic bismuth, comprising the following steps:

[0023] (1) melting a bismuth-containing raw material under an inert atmosphere to obtain a molten bismuth liquid;

[0024] (2) A phosphate impurity remover, an oxidant, and a molten bismuth solution are reacted under an inert atmosphere, and negative potential impurities in the molten bismuth solution are converted into phosphate scum, which is removed to obtain high-purity metallic bismuth.

[0025] The bismuth-containing raw material of the present invention is preferably a mixture of crude metallic bismuth and bismuth oxide or crude metallic bismuth with a bismuth grade of more than 95%; the negative potential impurity elements in the bismuth-containing raw material are preferably one or more of zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt, wherein the contents of zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, magnesium, and cobalt are independently preferably 0.0001 to 3%.

[0026] When the bismuth-containing raw material of the present invention is a mixture of crude metallic bismuth and bismuth oxide, the bismuth-containing raw material is preferably mixed with a reducing agent and then melted; the purpose of mixing the bismuth-containing raw material with the reducing agent is to reduce the bismuth oxide to metallic bismuth; the reducing agent is preferably carbon powder; the mass ratio of the reducing agent to the bismuth-containing raw material is preferably 1 to 10:100, more preferably 2 to 7:100, and even more preferably 3 to 5:100.

[0027] The melting temperature in step (1) of the present invention is preferably 400-1100°C, more preferably 600-1000°C, and more preferably 800-950°C; the melting time is preferably 50-200 min, more preferably 70-150 min, and more preferably 90-120 min.

[0028] The phosphate impurity remover in step (2) of the present invention is preferably one or more of bismuth phosphate, ammonium salt of phosphorus oxyacid and ammonium polyphosphate; the bismuth phosphate is preferably BiPO4; the ammonium salt of phosphorus oxyacid is preferably (NH4)3PO4, NH4PO3, (NH4)2HPO4 or NH4H2PO4; the ammonium polyphosphate is preferably (NH4,H)4P2O7, (NH4,H)5P3O 10 、(NH4,H)6P4O 13 , NH4H2PO2 or H 12 N3O3P; the amount of the phosphate impurity remover is preferably 1 to 10 times the theoretical amount, more preferably 3 to 7 times the theoretical amount, and more preferably 4 to 6 times the theoretical amount.

[0029] The oxidant in step (2) of the present invention preferably comprises one or more of NaNO3, NaNO2, Na2O2, KNO3, KNO2 and K2O2; the amount of the oxidant is preferably 0.1 to 3 times the theoretical amount, more preferably 0.2 to 2 times the theoretical amount, and more preferably 0.5 to 1.2 times the theoretical amount; the temperature of the reaction in step (2) is preferably 400 to 1100°C, more preferably 500 to 1000°C, and more preferably 700 to 900°C; the reaction time is preferably 30 to 300 min, more preferably 45 to 220 min, and more preferably 70 to 100 min.

[0030] The inert atmosphere in step (1) and step (2) of the present invention is preferably a nitrogen atmosphere and / or an argon atmosphere, and more preferably a nitrogen atmosphere.

[0031] In the impurity removal reaction of the present invention, the negative potential impurity element reacts with the phosphate impurity remover to form phosphate, or the negative potential impurity element first reacts with the oxidant to form an oxide, and the oxide then reacts with the phosphate impurity remover to form phosphate. The density of the phosphate generated by the reaction is lower than that of the molten bismuth solution, and the phosphate floats on the surface of the molten bismuth solution to form scum. The scum is removed to obtain high-purity metallic bismuth.

[0032] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0033] Example 1

[0034] A mixture of crude metallic bismuth and bismuth oxide was used as the bismuth-containing raw material. The bismuth grade of the raw material was 94.95%, of which the bismuth oxide content in the bismuth-containing phase was 48.31% and the crude metallic bismuth content was 51.69%. The negative potential impurities in the raw material were 0.0037% Zn, 0.0033% Mg, 0.066% Fe, 0.00055% As, 0.00072% Pb, 0.0012% Ni, 0.00012% Cd, 0.0016% Sn, and 0.00023% Cr. 30.00g of the mixture of metallic bismuth and bismuth oxide was weighed, 0.30g of carbon powder was added, and the mixture was melted under a nitrogen atmosphere at a melting temperature of 950°C for 90 minutes. Bismuth phosphate (BiPO4) and the oxidant (NaNO3) were added to a molten bismuth solution, with the BiPO4 dosage controlled at 1.2 times the theoretical amount and the NaNO3 dosage at 0.2 times the theoretical amount. The bismuth solution was stirred under a nitrogen atmosphere for a complete reaction at 900°C for 65 minutes. The scum was removed to obtain a high-purity metallic bismuth product. Testing revealed that the contents of negatively charged impurities in the high-purity metallic bismuth product were reduced to 0.000013% Zn, 0.000089% Mg, 0.000085% Fe, 0.000011% As, 0.000082% Pb, 0.000075% Ni, 0.000010% Cd, 0.000010% Sn, and 0.000090% Cr, respectively.

[0035] Example 2

[0036] Crude bismuth was used as the raw material. The bismuth grade of the bismuth-containing raw material was 97.68%, and the negative potential impurity contents were 0.052% Zn, 0.068% Mg, 0.236% Fe, 0.711% As, 0.0098% Pb, 0.0022% Ni, 0.00034% Cd, 1.237% Sn, and 0.00047% Cr. 30.00g of the crude bismuth was weighed and melted under a nitrogen atmosphere at a melting temperature of 750°C for 145 minutes. Ammonium oxyphosphate salt (NH₄H₂PO₄) and an oxidizing agent (Na₂O₂) were added to the molten bismuth solution, with the NH₄H₂PO₄ amount being 5 times the theoretical amount and the Na₂O₂ amount being 1.2 times the theoretical amount. The bismuth solution was stirred under a nitrogen atmosphere for thorough reaction at a temperature of 600°C for 220 minutes. The scum was removed to obtain a high-purity metallic bismuth product. The contents of negatively charged impurities in the product were reduced to 0.000011% Zn, 0.000081% Mg, 0.000072% Fe, 0.000010% As, 0.000078% Pb, 0.000072% Ni, 0.000010% Cd, 0.000010% Sn, and 0.000063% Cr, respectively.

[0037] Example 3

[0038] Crude bismuth was used as the raw material. The bismuth grade of the bismuth-containing raw material was 99.08%, and the contents of negative potential impurity elements were 0.233% Zn, 0.076% Mg, 0.039% Fe, 0.013% As, 0.089% Pb, 0.047% Ni, 0.0036% Cd, 0.448% Sn, 0.0032% Cr, and 0.033% Co. 50.00 g of the crude bismuth was weighed and melted under an argon atmosphere at a melting temperature of 1000°C for 120 minutes. Ammonium oxyphosphate (NH₄)₃PO₄) and an oxidizing agent, KNO₂, were added to a molten bismuth solution. The (NH₄)₃PO₄ amount was controlled to be 6.0 times the theoretical amount, and the KNO₂ amount was controlled to be 0.5 times the theoretical amount. The bismuth solution was stirred under an argon atmosphere for thorough reaction at a temperature of 800°C for 30 minutes. The scum was removed to obtain a high-purity metallic bismuth product. The contents of negatively charged impurities in the product were reduced to 0.000010% Zn, 0.000070% Mg, 0.000072% Fe, 0.000010%, 0.000049% Pb, 0.000070% Ni, 0.000010% Cd, 0.000010% Sn, 0.000010%, 0.000010% Cr, and 0.000065% Co, respectively.

[0039] Example 4

[0040] Crude bismuth was used as the raw material. The bismuth grade of the bismuth-containing raw material was 99.91%, and the contents of negative potential impurity elements were 0.0072% Zn, 0.0082% Mg, 0.053% Fe, 0.00050% As, 0.0028% Pb, 0.0036% Ni, 0.00027% Cd, 0.0022% Sn, and 0.0031% Cr. 50.00 g of the crude bismuth raw material was weighed and melted under a nitrogen atmosphere at 900° C. for 130 minutes. Ammonium polyphosphate (NH4,H)4P2O7 and an oxidant, KNO3, were added to a molten bismuth solution. The (NH4,H)4P2O7 dosage was controlled to be 4 times the theoretical dosage, and the KNO3 dosage was controlled to be 0.5 times the theoretical dosage. The bismuth solution was stirred under a nitrogen atmosphere for thorough reaction at a temperature of 750°C for 45 minutes. The scum was removed to obtain a high-purity metallic bismuth product. The contents of negatively charged impurities in the product were reduced to 0.000010% for Zn, 0.000060% for Mg, 0.000055% for Fe, 0.000010% for As, 0.000045% for Pb, 0.000062% for Ni, 0.000010% for Cd, 0.000010% for Sn, and 0.000010% for Cr, respectively.

[0041] Comparative Example 1

[0042] YUYAN Technology Group Co., Ltd. and Kunming University of Science and Technology [Ding Weian, Niu Huixian, Dai Yongnian. Vacuum refining of silver-containing crude bismuth [J]. Vacuum Science and Technology, 1998, (02): 155-160.] used vacuum distillation to refine crude bismuth. The main chemical components and contents of crude bismuth were: Bi 98.38%, Ag 0.6914%, Pb 0.077%, Fe 0.065%, Cu 0.012%. After three-stage vacuum distillation test, the lead content of the refined bismuth was 0.0090% to 0.0095%.

[0043] Compared with the examples of the present invention, comparative example 1, after three vacuum distillations using the vacuum distillation method, still failed to meet the lead impurity limit requirement of Bi99.999 (YS / T818-2012). The high-purity metallic bismuth obtained by the present invention through a single impurity removal meets the impurity limit requirement of Bi99.999 (YS / T818-2012).

[0044] Comparative Example 2

[0045] Shandong Hengbang Smelting Co., Ltd. [Zhang Weijie, Wang Ruiqiang. Application of vacuum distillation furnace in the production process of refined bismuth [J]. World Nonferrous Metals, 2021, (18): 15-17.] The refining process adopted is as follows: bismuth slag is reduced and removed by adding coke and soda ash in a converter to produce crude bismuth. The crude bismuth is heated and melted in a bismuth pot and then cooled and smelted to remove copper. Compressed air is introduced for oxidation to remove arsenic, antimony, and tellurium. Alkali is added to further remove arsenic and tellurium. Then chlorine is introduced for chlorination to remove lead. After lead removal is completed, the alloy enters a vacuum distillation furnace for vacuum distillation to remove silver. The refined bismuth alloy produced is finally refined to further remove lead, antimony, etc., so that the impurity element content is qualified and then cast into ingots to produce 1# bismuth ingots that meet national standards.

[0046] Compared with the embodiment of the present invention, the comparative example 2 required cumber removal by smelting, oxidative scouring, and lead removal by chlorination before vacuum distillation refining, which was a complex process. The present invention, by adding a phosphate impurity remover and an oxidizing agent, can remove all negative potential metal impurities in one step, meeting the impurity limit requirements of the Bi99.999 (YS / T818-2012) standard.

[0047] Comparative Example 3

[0048] Yao Li [Yao Li. Purification of metallic bismuth by zone melting [J]. Chemical World, 1981, (08): 3-4.] After pretreatment, industrial bismuth raw materials were placed in a quartz boat and reduced into ingots in a two-stage furnace. The reduced bismuth ingots and the quartz boat were placed in a quartz tube and placed on a zone melting furnace. Zone melting was repeated 20 to 27 times. The ingots after zone melting were divided into three sections, the first and middle sections were merged, and the tail end of the bismuth ingot with concentrated impurities was discarded to obtain 99.999% refined bismuth.

[0049] Compared with the embodiment of the present invention, the comparative example 3 adopts the zone melting method and performs zone melting 20 to 27 times to obtain 5N metallic bismuth, and the production efficiency is significantly lower. The preparation method of the present invention is easy to industrialize and has high production efficiency.

[0050] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing high-purity metallic bismuth, It is characterized in that The following steps are included: (1) melting a bismuth-containing raw material under an inert atmosphere to obtain a molten bismuth liquid; (2) reacting a phosphate impurity remover, an oxidant, and a molten bismuth solution under an inert atmosphere, wherein negative potential impurities in the molten bismuth solution generate phosphate scum, and removing the phosphate scum to obtain high-purity metallic bismuth; The negative potential impurity elements in the bismuth-containing raw material in step (1) include zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, and magnesium, wherein the contents of zinc, lead, nickel, arsenic, iron, cadmium, tin, chromium, and magnesium are independently 0.0001 to 3%; Step (2) The oxidant comprises NaNO 3 、NaNO 2 、Na 2 O 2 、KNO 3 、KNO 2 and K 2 O 2 One or more of the following; the amount of the oxidant is 0.1 to 3 times the theoretical amount; The reaction temperature in step (2) is 600-1100° C. and the reaction time is 30-300 min.

2. The preparation method according to claim 1, It is characterized in that The bismuth-containing raw material in step (1) comprises a mixture of crude metallic bismuth and bismuth oxide or crude metallic bismuth with a bismuth grade of more than 95%.

3. The preparation method according to claim 2, It is characterized in that In step (1), when the bismuth-containing raw material is a mixture of crude metallic bismuth and bismuth oxide, the bismuth-containing raw material is mixed with a reducing agent and then melted; the reducing agent is carbon powder; and the mass ratio of the reducing agent to the bismuth-containing raw material is 1 to 10:

100.

4. The preparation method according to claim 1, It is characterized in that The melting temperature in step (1) is 400-1100° C. and the melting time is 50-200 min.

5. The preparation method according to claim 1 or 4, It is characterized in that The phosphate impurity remover in step (2) comprises one or more of bismuth phosphate, ammonium salt of phosphorus oxyacid and ammonium polyphosphate; the bismuth phosphate is BiPO 4 ; The phosphorus oxyacid ammonium salt is (NH 4 ) 3 PO 4 NH 4 PO 3 NH 4 ) 2 HPO 4 or NH 4 H 2 PO 4 ; The ammonium polyphosphate is (NH 4 ,H) 4 P 2 O 7 NH 4 ,H) 5 P 3 O 10 or (NH 4 ,H) 6 P 4 O 13 .

6. The preparation method according to claim 5, It is characterized in that The dosage of the phosphate impurity remover in step (2) is 1 to 10 times the theoretical dosage.

7. The preparation method according to claim 1, It is characterized in that The inert atmosphere in step (1) and step (2) is a nitrogen atmosphere and / or an argon atmosphere.

Citation Information

Patent Citations

  • Process for removing Pb and Zn from raw Bi

    CN1124783A