A bismuth sulfide semiconductor material with high electrical conductivity and its preparation method and application

Through hydrothermal reaction method and discharge plasma calcining process, a high-conductivity bismuth sulfide semiconductor material was prepared, which solved the problem of low conductivity in the prior art, achieved efficient conductivity under high temperature conditions, and improved its photoelectricity Application performance in the fields of thermoelectricity and other fields.

CN115974151BActive Publication Date: 2024-11-19XIAN TIANJICHENG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310178471.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-11-19
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

In the prior art, the conductivity of bismuth sulfide semiconductor materials is relatively low, which limits its further development and application in the fields of semiconductor energy conversion materials, photovoltaics, photovoltaics, thermoelectrics and batteries.

Method used

Hydrothermal reaction method is used to mix thiourea with bismuth nitrate solution, and then conduct hydrothermal reaction and discharge plasma calcination to prepare bismuth sulfide semiconductor material with high conductivity, avoiding the addition of other substances to reduce the reduction of free S2- , simplify the process and reduce costs.

Benefits of technology

In the range of 323 to 523K, the conductivity of bismuth sulfide semiconductor material reaches 25 to 32S/cm, which is significantly higher than the prior art, improves carrier concentration and mobility, enhances the sensitivity of photoelectric sensors and the refrigeration of thermoelectric devices Or power generation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974151B_ABST
    Figure CN115974151B_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth sulfide semiconductor material with high electrical conductivity and a preparation method and application thereof, belonging to the technical field of semiconductor material synthesis. Thiourea and bismuth nitrate pentahydrate are firstly subjected to hydrothermal reaction, and then calcined to obtain the bismuth sulfide semiconductor material with high electrical conductivity. Compared with other methods, the hydrothermal reaction has easy-to-obtain equipment and raw materials, a simple process, low energy consumption, and a small product particle size. After discharge plasma sintering, temperature and pressure changes can be achieved simultaneously, and the temperature can be rapidly increased in a short time to avoid secondary growth of grains during the heating process. The obtained bismuth sulfide semiconductor material with high electrical conductivity has more excellent electrical conductivity, and within the range of 323 to 523 K, the electrical conductivity reaches 25 to 32 S / cm, which is much higher than the electrical conductivity of the bismuth sulfide semiconductor material in the prior art. The bismuth sulfide semiconductor material has good application prospects in photoelectric sensors, photoelectric detectors, photodiodes, high-temperature spacecraft ultra-long life power supplies, self-powered sensors and thermoelectric devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor material synthesis, and specifically relates to a bismuth sulfide semiconductor material with high electrical conductivity, a preparation method and an application thereof. Background Art

[0002] According to the different conductivity, materials in nature can be divided into three categories: conductors, semiconductors, and insulators. Semiconductor materials refer to electronic materials with semiconductor properties that may be used to make semiconductor devices. In recent years, with the continuous development of the field of semiconductor materials, sulfides, especially binary sulfides (Bi2S3, PbS, CdS, and Ag2S, etc.), have been widely used in semiconductor energy conversion materials and devices (such as optoelectronics, photovoltaics, thermoelectrics, and batteries, etc.), chemistry (catalysis and photoluminescence) and electrochemistry (electrochemical sensors, etc.) due to their unique physical and chemical properties, low price, high abundance of elements contained, and environmental friendliness.

[0003] Bismuth sulfide (Bi2S3) is a semiconductor material of group V-VI, with unit cell parameters a=1.1149nm, b=1.1304nm, c=0.3981nm, band gap energy of 1.33eV at room temperature, and energy band gap of 1.3~1.7eV, which belongs to direct band gap semiconductor material. Bismuth sulfide semiconductor material is widely used in photoelectric sensors, photodetectors, thermoelectric devices and photodiode arrays due to its unique advantages such as excellent photoelectric effect, nonlinear optical response, thermoelectric effect and visible light absorption. Ge et al. prepared pure phase bismuth sulfide semiconductor material by mechanical alloying method, and its conductivity only fluctuated between 4~12S / cm in the temperature range of 323K~573K (Ge ZH, Zhang BP, Liu Y, et al. Nanostructured Bi 2-x Cu x S3 bulk materials with enhanced thermoelectric performance[J].Physical Chemistry Chemical Physics,2012,14(13):4475-4481.);Yang et al. prepared pure phase bismuth sulfide semiconductor materials by vacuum melting method, and the maximum conductivity was only 5S / cm in the temperature range of 323~723K (Yang J,Yu L,Wang T,et al.Thermoelectric properties of n-typeCu xBi2S3materials fabricated by plasma activated sintering[J].Journal ofAlloysandCompounds,2019,780:35-40.); Zhao et al. synthesized bismuth sulfide semiconductor materials by solvothermal method. In order to improve the conductivity, in addition to adding Bi source and S source, they also added KBr and PVP. They regulated the morphology of cotton-like bismuth sulfide materials formed by the accumulation of nanowires with a diameter of about 10nm. In the temperature range of 323-523K, the maximum conductivity was 20S / cm (Zhao W, Jin K, Fu L, et al. Mass Production of Pt Single-Atom-Decorated Bismuth Sulfide for n-Type Environmentally Friendly Thermoelectrics[J].Nano Letters, 2022, 22(12): 4750-4757.); Guo et al. added thioacetic acid as an additive in the process of hydrothermal synthesis of pure bismuth sulfide, and prepared curved rod-shaped bismuth sulfide composed of thin sheets by controlling the morphology to construct a new conductive network. In the temperature range of 323-523K, the conductivity was less than 10S / cm (Guo J, Yang J, Ge ZH, et al. Realizing high thermoelectric performance in earth-abundant Bi2S3 bulkmaterials via halogen acid modulation[J]. Advanced Functional Materials, 2021, 31(37): 2102838.).

[0004] The bismuth sulfide prepared by the above experimental method has low electrical conductivity, which seriously limits the further development and application of bismuth sulfide semiconductor materials in the fields of semiconductor energy conversion materials, optoelectronic, photovoltaic, thermoelectric and battery devices, catalytic chemistry, photoluminescent materials, electrochemical sensors, etc. It is necessary to carry out modification research to improve the electrical conductivity of bismuth sulfide semiconductor materials. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a bismuth sulfide semiconductor material with high conductivity and a preparation method and application thereof, so as to solve the technical problem of low conductivity of bismuth sulfide semiconductor materials in the prior art.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for preparing a bismuth sulfide semiconductor material with high electrical conductivity, comprising: adding thiourea to a bismuth nitrate pentahydrate solution, stirring sufficiently, firstly performing a hydrothermal reaction, cooling to room temperature, centrifuging, drying, and performing discharge plasma calcination to obtain the bismuth sulfide semiconductor material with high electrical conductivity.

[0008] Preferably, the experimental raw materials only involve thiourea and bismuth nitrate pentahydrate, and no other substances are added during the experiment. The mass ratio of thiourea: bismuth nitrate pentahydrate is (1.03-1.568): (2.51-3.11).

[0009] Preferably, the bismuth nitrate pentahydrate solution is prepared by dissolving 2.51 to 3.11 g of bismuth nitrate pentahydrate in 60 to 80 mL of distilled water and stirring at room temperature for 5 to 20 minutes.

[0010] Preferably, the temperature of the hydrothermal reaction is 100-160°C.

[0011] Preferably, the hydrothermal reaction time is 8 to 16 hours.

[0012] Preferably, the calcination pressure is 30-50 MPa, the calcination temperature is 300-500° C., and the holding time is 2-20 min.

[0013] Preferably, the stirring conditions are: stirring for 10 to 20 minutes, ultrasonic dispersion for 15 to 30 minutes, and stirring again for 15 to 30 minutes.

[0014] Preferably, the drying temperature is 70° C. and the drying time is 12 h.

[0015] The invention also discloses a bismuth sulfide semiconductor material with high conductivity obtained by the preparation method, wherein the conductivity reaches 25 to 32 S / cm in the range of 323 to 523 K.

[0016] The present invention also discloses the use of the above-mentioned bismuth sulfide semiconductor material with high conductivity in the preparation of photoelectric sensors, photoelectric detectors, photodiodes, high-temperature spacecraft ultra-long life power supplies, self-powered sensors and thermoelectric device materials.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention discloses a method for preparing a bismuth sulfide semiconductor material with high electrical conductivity. Thiourea is mixed with a bismuth nitrate pentahydrate solution without adding any other substances. After sufficient stirring, a hydrothermal reaction is first performed. The hydrothermal reaction experimental equipment and raw materials are easy to obtain, the process is simple, the energy consumption is low, and the product particle size is small. Then, discharge plasma calcination is performed. The discharge plasma calcination can not only achieve temperature and pressure changes at the same time, but also can quickly heat up in a short time, avoiding the secondary growth of grains during the heating process, and obtaining a bismuth sulfide semiconductor material with high electrical conductivity. Compared with bismuth sulfide semiconductor materials prepared by other methods, the bismuth sulfide semiconductor material with high electrical conductivity prepared by the present invention does not add other additives during the preparation process, avoiding excessive S 2- Free, excess S in solution 2- It is easy to be reduced to S element during the hydrothermal reaction, and trace amounts of S element will also have a negative effect on the overall conductivity of bismuth sulfide. Moreover, experimental equipment and chemical reagents are easy to obtain, the process conditions are simple, the operation is simple, the cost is low, the yield is high, and the industrial application value is high. In the range of 323-523K, the maximum conductivity is 32S / cm.

[0019] Furthermore, the mass ratio of thiourea to bismuth nitrate pentahydrate is (1.03-1.568):(2.51-3.11), that is, the molar ratio of thiourea to bismuth nitrate pentahydrate is (0.014-0.02):(0.0052-0.0064).

[0020] Furthermore, the bismuth nitrate pentahydrate solution is prepared by dissolving 2.51 to 3.11 g of bismuth nitrate pentahydrate in 60 to 80 mL of distilled water. A higher concentration of the bismuth nitrate pentahydrate solution can not only obtain a pure phase of bismuth sulfide semiconductor material but also greatly increase the yield of bismuth sulfide synthesized by hydrothermal reaction.

[0021] The invention also discloses a bismuth sulfide semiconductor material with high conductivity obtained by the preparation method. The conductivity of the bismuth sulfide semiconductor material is 25 to 32 S / cm in the range of 323 to 523 K, which is much higher than the conductivity of the bismuth sulfide semiconductor material in the prior art.

[0022] The present invention also discloses the use of the above-mentioned bismuth sulfide semiconductor material with high conductivity in the preparation of photoelectric sensors, photoelectric detectors, photodiodes, ultra-long life power supplies for high-temperature spacecraft, self-powered sensors and thermoelectric device materials. When the bismuth sulfide semiconductor material prepared by the present invention is used in the above-mentioned fields, it can provide higher carrier concentration and mobility to obtain good conductivity. When used in devices such as photoelectric sensors, photodetectors, photodiodes, etc., it has stronger sensitivity to light signals; when used in ultra-long life power supplies and self-powered sensors for high-temperature spacecraft, it is beneficial to the electron transfer process; when used in thermoelectric devices, under the same temperature difference, a better refrigeration or power generation effect can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD diagram of the product obtained after hydrothermal reaction treatment in Example 1 of the present invention;

[0024] Figure 2 This is a conductivity diagram of the bismuth sulfide semiconductor material with high conductivity prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0026] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0027] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0028] The present invention provides a method for preparing a bismuth sulfide semiconductor material with high electrical conductivity, comprising the following steps:

[0029] Step 1) Weigh 2.51-3.11 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 60-80 mL of distilled water. Stir for 5-20 min at room temperature to obtain a milky white solution A.

[0030] Step 2) Add 1.03-1.568 g of thiourea (CH4N2S) to the solution A obtained in step 1), continue stirring for 10-20 min to obtain an orange solution B, then ultrasonically disperse it for 15-30 min, and stir again for 15-30 min;

[0031] Step 3) The solution obtained in step 2) is placed in a reactor for hydrothermal reaction at a temperature of 100 to 160° C. for 8 to 16 hours. After the reaction is completed, the solution is cooled to room temperature, centrifuged, and dried in an oven at 70° C. for 12 hours to obtain a powder product C.

[0032] Step 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 300-500° C., a sintering pressure of 30-50 MPa, and a heat preservation time of 2-20 min, to finally obtain a bulk bismuth sulfide material.

[0033] The preparation process of the present invention is simple and low-cost, and the conductivity of the bismuth sulfide semiconductor material is effectively improved. Compared with other methods, the bismuth sulfide prepared by the hydrothermal method is subjected to spark plasma sintering to obtain a bismuth sulfide semiconductor material with high conductivity, and the maximum conductivity is 32S / cm in the range of 323 to 523K.

[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0037] 1) Weigh 2.896 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0038] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 15 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0039] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 120° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0040] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 38 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0041] The bismuth sulfide material prepared in this embodiment has an electrical conductivity of 32 S / cm at 423K after being tested by a precision potential test system.

[0042] See also Figure 1 This is the XRD diagram of the product obtained after the hydrothermal reaction treatment in Example 1; it can be seen from the figure that the diffraction peaks of the sample can correspond to the standard card PDF#17-0320, no diffraction peaks of other impurities appear, and all diffraction peaks are relatively sharp, indicating that the sample has good crystallinity.

[0043] See also Figure 2 This is a conductivity diagram of the bismuth sulfide thermoelectric material prepared in this Example 1; it can be seen from the figure that the conductivity shows a trend of first increasing and then decreasing with increasing temperature, and the maximum conductivity of 32S / cm is obtained at 423K. The conductivity has a downward trend after the temperature increases, which may be because at high temperatures, the electron scattering effect is enhanced, resulting in a decrease in conductivity.

[0044] Example 2

[0045] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0046] 1) Weigh 2.51 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 60 mL of distilled water. Stir for 10 min at room temperature to obtain a milky white solution A.

[0047] 2) adding 1.03 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 10 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0048] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 100° C. for 8 h. After the reaction is completed, cooling to room temperature, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0049] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 300-500° C., a sintering pressure of 30 MPa, and a holding time of 2 min, to finally obtain a bulk bismuth sulfide material.

[0050] The bismuth sulfide material prepared in this example has an electrical conductivity of 25 S / cm at 473K after being tested by a precision potential test system.

[0051] Example 3

[0052] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0053] 1) Weigh 3.11 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 80 mL of distilled water. Stir for 20 min at room temperature to obtain a milky white solution A.

[0054] 2) adding 1.568 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 20 min to obtain an orange solution B, which was then ultrasonically dispersed for 30 min and stirred again for 30 min;

[0055] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 160° C. for 16 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0056] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 500° C., a sintering pressure of 50 MPa, and a holding time of 20 min, to finally obtain a bulk bismuth sulfide material.

[0057] The bismuth sulfide material prepared in this embodiment has an electrical conductivity of 27 S / cm at 523K after being tested by a precision potential test system.

[0058] Example 4

[0059] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0060] 1) Weigh 2.896 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0061] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 15 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0062] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 160° C. for 12 h. cooling to room temperature after the reaction, centrifugally drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0063] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 40 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0064] The bismuth sulfide material prepared in this example was tested by a precision potential test system and showed that it had an electrical conductivity of 26 S / cm at 473K.

[0065] Example 5

[0066] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0067] 1) Weigh 2.88 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0068] 2) adding 1.348 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 20 min to obtain an orange solution B, which was then ultrasonically dispersed for 15 min and stirred again for 15 min;

[0069] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 120° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0070] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 40 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0071] The bismuth sulfide material prepared in this example was tested by a precision potential test system and showed that it had an electrical conductivity of 28 S / cm at 423K.

[0072] Example 6

[0073] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0074] 1) Weigh 2.896 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 20 min at room temperature to obtain a milky white solution A.

[0075] 2) adding 1.378 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 15 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0076] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 130° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0077] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 35 MPa, and a holding time of 5 min, to finally obtain a doped bulk bismuth sulfide material.

[0078] The bismuth sulfide material prepared in this embodiment has an electrical conductivity of 25 S / cm at 523K after being tested by a precision potential test system.

[0079] Example 7

[0080] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0081] 1) Weigh 2.88 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0082] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 20 min to obtain an orange solution B, which was then ultrasonically dispersed for 15 min and stirred again for 15 min;

[0083] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a reaction temperature of 110° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0084] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 40 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0085] The bismuth sulfide material prepared in this example has an electrical conductivity of 28 S / cm at 473K after being tested by a precision potential test system.

[0086] Example 8

[0087] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0088] 1) Weigh 2.896 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0089] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 15 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0090] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 120° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0091] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 35 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0092] The bismuth sulfide material prepared in this example has an electrical conductivity of 28 S / cm at 473K after being tested by a precision potential test system.

[0093] Example 9

[0094] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0095] 1) Weigh 2.88 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 20 min at room temperature to obtain a milky white solution A.

[0096] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 20 min to obtain an orange solution B, which was then ultrasonically dispersed for 15 min and stirred again for 15 min;

[0097] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 140° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0098] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 450° C., a sintering pressure of 30 MPa, and a holding time of 5 min, to finally obtain a bulk bismuth sulfide material.

[0099] The bismuth sulfide material prepared in this example has an electrical conductivity of 27 S / cm at 473K after being tested by a precision potential test system.

[0100] Example 10

[0101] A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity comprises the following steps:

[0102] 1) Weigh 2.896 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and dissolve it in 70 mL of distilled water. Stir for 15 min at room temperature to obtain a milky white solution A.

[0103] 2) adding 1.368 g of thiourea (CH4N2S) to the solution A obtained in step 1), and continuing stirring for 15 min to obtain an orange solution B, which was then ultrasonically dispersed for 20 min and stirred again for 20 min;

[0104] 3) placing the solution obtained in step 2) into a reactor for hydrothermal reaction at a temperature of 120° C. for 12 h. cooling to room temperature after the reaction, centrifugation drying, and drying in an oven at 70° C. for 12 h to obtain a powder product C;

[0105] 4) placing the product C obtained in step 3) into a spark plasma sintering mold, with a sintering temperature of 400° C., a sintering pressure of 40 MPa, and a holding time of 15 min, to finally obtain a bulk bismuth sulfide material.

[0106] The bismuth sulfide material prepared in this example has an electrical conductivity of 28 S / cm at 523K after being tested by a precision potential test system.

[0107] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a bismuth sulfide semiconductor material with high electrical conductivity, characterized in that: include: Thiourea is added to a bismuth nitrate pentahydrate solution, and after sufficient stirring, a hydrothermal reaction is first performed, the solution is cooled to room temperature, centrifuged, dried, and subjected to discharge plasma calcination to obtain a bismuth sulfide semiconductor material having high electrical conductivity; In the range of 323-523 K, the conductivity of the high-conductivity bismuth sulfide semiconductor material reaches 25-32 S / cm; The experimental raw materials only involve thiourea and bismuth nitrate pentahydrate, and no other substances are added during the experiment. The mass ratio of thiourea: bismuth nitrate pentahydrate is (1.03~1.568): (2.51~3.11); The bismuth nitrate pentahydrate solution is prepared by dissolving 2.51-3.11 g of bismuth nitrate pentahydrate in 60-80 mL of distilled water and stirring at room temperature for 5-20 min; The temperature of the hydrothermal reaction is 100-130°C; the time of the hydrothermal reaction is 8-16 hours; The calcination pressure is 30-50 MPa, the calcination temperature is 300-500°C, and the insulation time is 2-20 min.

2. The method for preparing a bismuth sulfide semiconductor material with high electrical conductivity according to claim 1, characterized in that: The stirring conditions are as follows: stirring for 10 to 20 min, ultrasonic dispersion for 15 to 30 min, and stirring again for 15 to 30 min.

3. The method for preparing a bismuth sulfide semiconductor material with high electrical conductivity according to claim 1, characterized in that: The drying temperature is 70°C and the drying time is 12 h.

4. A bismuth sulfide semiconductor material with high electrical conductivity obtained by the preparation method according to any one of claims 1 to 3.

5. Use of the bismuth sulfide semiconductor material with high electrical conductivity as claimed in claim 4 in the preparation of photoelectric sensors, photodetectors, photodiodes, high-temperature spacecraft ultra-long life power supplies, self-powered sensors and thermoelectric device materials.