Catalyst component for ethylene polymerization, catalyst and ethylene polymerization reaction method
By mixing magnesium compounds with organic epoxy compounds, etc. and reacting with non-polar solvents, combining organic aluminum compounds, the activity of ethylene polymerization catalyst is improved, and the existing problems of low catalyst activity and poor polymer particle size distribution are solved, so as to achieve Preparation of polymers with high bulk density and concentrated particle size distribution is performed.
Patent Information
- Application Number
- CN202111201007.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-14
AI Technical Summary
The existing ethylene polymerization catalyst has low activity, wide particle size distribution of polymers, and poor particle shape, making it difficult to obtain polymers with high bulk density and concentrated particle size distribution.
Magnesium compounds, organic epoxy compounds, organic phosphorus compounds, organic alcohol compounds and polar diluents are used to form a uniform solution, and react with non-polar solvents and titanium compounds. Catalyst components are precipitated by heating and precipitation, and organic aluminum compounds are added. To improve catalyst activity, polymerization of ethylene or ethylene with α-olefin is carried out.
The catalyst activity was significantly improved, and the obtained polymer had high bulk density, spherical shape and concentrated particle size distribution, with good particle shape and particle size distribution.
Smart Images

Figure BDA0003304462260000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ethylene polymerization, and more specifically, relates to a catalyst component and a catalyst for ethylene polymerization, and an ethylene polymerization reaction method. Background Art
[0002] In the polymerization of olefins, especially the polymerization of ethylene or the copolymerization of ethylene and α-olefins, catalyst components having magnesium, titanium, halogen and electron donor as essential components are often used.
[0003] In fact, the above catalyst components are mainly composed of magnesium chloride, titanium chloride and electron donors. The early catalyst components mixed and ground magnesium chloride, titanium tetrachloride and electron donors together. This type of catalyst has low activity, and the prepared polymer particle size distribution is very wide, with more coarse powder and fine powder. It is now basically eliminated.
[0004] One is to load the catalyst components on a porous spherical silica gel in a fixed form. For example, patent document CN1158136 discloses a main catalyst for producing ethylene polymers, which includes an inorganic carrier (preferably an active silica carrier), a chlorine compound supported on the carrier, a magnesium compound supported on the carrier, and a titanium compound supported on the carrier. The main catalyst is characterized in that the catalyst particles are spherical, have good fluidity, good hydrogen sensitivity, and the polymerization activity decreases less with the increase in the amount of chain transfer agent (hydrogen) added, and is more suitable for producing polyethylene resins with a wide molecular weight distribution.
[0005] The other method is to dissolve the magnesium compound into a uniform solution, and then react it with a titanium compound to precipitate magnesium chloride particles while loading titanium chloride and electron donors, such as disclosed in patent documents CN85100997, CN1112373C, CN1229092A, CN1958620, etc. This method generally dissolves the magnesium compound in a polar solvent, and the dissolved solution is contacted with titanium tetrachloride to precipitate catalyst component particles containing titanium magnesium and electron donors. This method is simple and easy to implement, and the performance of the catalyst component is much better than that of the mixed and ground catalyst.
[0006] In patent document CN85100997, magnesium halide is dissolved in organic epoxy compound and organic phosphorus compound to form a uniform solution, and then reacted with at least one precipitation aid and transition metal titanium halide and its derivatives to prepare. Because organic epoxy compound and organic phosphorus compound without active hydrogen are used as solvents, they dissolve magnesium chloride slowly, and the reaction with titanium tetrachloride is easy to control, so the precipitated particles have better shape, which is spherical, and the prepared polymer has better particle shape and higher bulk density.
[0007] In patent document CN1112373C, magnesium chloride is dissolved in isooctyl alcohol with decane as dispersant, and then silane is added as precipitation agent, and the catalyst component particles are prepared by reaction with titanium tetrachloride. The solvent used in this system is isooctyl alcohol, the raw materials are simple, the catalyst component has high activity in ethylene polymerization, and the hydrogen regulation performance is good.
[0008] Patent document CN1229092A discloses a catalyst for ethylene polymerization or copolymerization, which is prepared by dissolving magnesium halide in organic epoxy compounds and organic phosphorus compounds and then adding a low-carbon alcohol as an electron donor activator to form a uniform solution, and then reacting with at least one acid anhydride precipitation aid and a transition metal titanium halide and its derivatives. The catalyst shows high activity when used for slurry polymerization of ethylene.
[0009] Patent document CN1958620 discloses a catalyst prepared by dissolving magnesium halide in an organic epoxy compound, an organic phosphorus compound and a low-carbon alcohol to form a uniform solution, and then reacting the solution with at least one silane compound and a halide of transition metal titanium and its derivatives. The catalyst has high activity when used for slurry polymerization of ethylene and the particle shape of the catalyst is improved. Summary of the invention
[0010] In view of the above situation, the purpose of the present invention is to provide a catalyst component for ethylene polymerization, a catalyst and an ethylene polymerization reaction method. The polymer prepared by using the catalyst of the present invention has a higher bulk density, a higher polymer sphericity, a concentrated polymer particle size distribution, and a better polymer particle shape and particle size distribution.
[0011] A first aspect of the present invention provides a catalyst component for ethylene polymerization, wherein the preparation method of the catalyst component comprises:
[0012] 1) mixing a magnesium compound, an organic epoxy compound, an organic phosphorus compound, an organic alcohol compound and a polar diluent, stirring and reacting to obtain a uniform solution;
[0013] 2) contacting the uniform solution with a non-polar solvent and a titanium compound to react, precipitating solid particles by heating, washing to obtain a catalyst component or making it into a suspension.
[0014] A second aspect of the present invention provides a catalyst for ethylene polymerization, which comprises the above-mentioned catalyst component and an organic aluminum compound.
[0015] The third aspect of the present invention provides an ethylene polymerization method, which comprises: reacting ethylene or ethylene with α-olefin in the presence of the above-mentioned catalyst.
[0016] The catalyst component of the present invention is added with a non-polar solvent during the preparation process, and the obtained catalyst component has significantly higher activity, higher polymer bulk density, higher polymer sphericity, concentrated polymer particle size distribution, and better polymer particle shape and particle size distribution.
[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0019] According to a first aspect of the present invention, the present invention provides a catalyst component for ethylene polymerization, the preparation method of the catalyst component comprising:
[0020] 1) mixing a magnesium compound, an organic epoxy compound, an organic phosphorus compound, an organic alcohol compound and a polar diluent, stirring and reacting to obtain a uniform solution;
[0021] 2) contacting the uniform solution with a non-polar solvent and a titanium compound to react, precipitating solid particles by heating, washing to obtain a catalyst component or making it into a suspension.
[0022] According to the present invention, adding a non-polar solvent during the preparation of the catalyst component can improve the catalyst activity, increase the bulk density and sphericity of the polymer, and concentrate the polymer particle size distribution. The non-polar solvent and the titanium compound can react with the uniform solution separately or simultaneously.
[0023] Preferably, the contact reaction of the homogeneous solution with the non-polar solvent and the titanium compound is carried out in any of the following ways:
[0024] Method 1: Add a non-polar solvent to a uniform solution at 30-60°C, then cool to -30°C to 20°C, and add a titanium compound for contact reaction;
[0025] Method 2: Cooling the homogeneous solution to -30°C to 20°C, and then adding a non-polar solvent and a titanium compound into the homogeneous solution for contact reaction;
[0026] Method 3: adding a non-polar solvent to a uniform solution at 30-60°C, and then adding the obtained mixture to a titanium compound at a temperature of -30°C to 20°C for contact reaction.
[0027] In the present invention, the magnesium compound can be a magnesium-containing compound known to those skilled in the art, such as a magnesium halide, a magnesium alcoholate or a magnesium halogenated alcoholate, etc. Preferably, the magnesium compound is a magnesium dihalide or a derivative in which one halogen atom in the magnesium dihalide molecular formula is replaced by a hydrocarbon group or a halohydrocarbonoxy group.
[0028] According to the present invention, the organic epoxy compound is selected from aliphatic olefins, dienes, halogenated aliphatic olefins, oxides, glycidyl ethers or internal ethers of dienes having 2 to 8 carbon atoms, and is preferably at least one of ethylene oxide, propylene oxide, butylene oxide, butadiene oxide, butadiene dioxide, epichlorohydrin, methyl glycidyl ether and diglycidyl ether.
[0029] According to the present invention, the organophosphorus compound can be selected from the group consisting of hydrocarbyl esters or halogenated hydrocarbyl esters of orthophosphoric acid, hydrocarbyl esters or halogenated hydrocarbyl esters of phosphorous acid, for example, trimethyl orthophosphate, triethyl orthophosphate, tributyl orthophosphate, triphenyl orthophosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite, benzyl phosphite, etc.
[0030] According to the present invention, the organic alcohol compound can be selected from a linear alcohol or isomeric alcohol having 1 to 8 carbon atoms. Specific examples of organic alcohol compounds include, but are not limited to, at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-octanol and isooctanol. Preferably, it is a linear alcohol or isomeric alcohol having 3 to 8 carbon atoms.
[0031] In the present invention, the polar diluent may be benzene, toluene, xylene, chlorobenzene or derivatives thereof.
[0032] According to the present invention, the non-polar diluent may be hexane, heptane, octane or decane.
[0033] According to the present invention, the general formula of the titanium compound is Ti(OR) a X b , where R is C1-C 14 An aliphatic hydrocarbon group or an aromatic hydrocarbon group, X is a halogen atom, a is an integer from 0 to 2, b is an integer from 0 to 4, and a+b=3 or 4.
[0034] Specifically, the titanium compound can be at least one of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium trichloride, titanium triethoxide, titanium trichloride, titanium trichloride, titanium trichloride, titanium tetra ...
[0035] According to the present invention, per mole of magnesium compound, the amount of the organic epoxy compound is 0.01-10 moles, preferably 0.02-4 moles; the amount of the organic phosphorus compound is 0.01-10 moles, preferably 0.02-4 moles; the amount of the organic alcohol compound is 0.01-15 moles, preferably 0.05-10 moles; the amount of the polar diluent is 0.2-5L; the amount of the non-polar diluent is 0.2-5L; the amount of the titanium compound is 0.2-30 moles, preferably 1-20 moles.
[0036] Preferably, in step 1), the stirring speed is 350-500 rpm, the reaction temperature is 50-100° C., and the reaction time is 0.5-1.5 h.
[0037] Preferably, in step 2), the heating temperature is 60-110°C.
[0038] In the present invention, the solvent for preparing the suspension can be straight-chain or branched alkane, such as hexane, heptane, octane, decane or their derivatives.
[0039] According to a second aspect of the present invention, there is provided a catalyst for ethylene polymerization, the catalyst comprising the above-mentioned catalyst component and an organic aluminum compound.
[0040] In the present invention, the general formula of the organoaluminum compound can be AlR 1 n X 3-n , where R 1 is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, preferably an alkyl group, an aralkyl group or an aryl group; X is a halogen, preferably chlorine or bromine; and n is a number of 0<n≤3.
[0041] Specifically, the organoaluminum compound can be trimethylaluminum, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum monohydrogenate, diisobutylaluminum monohydrogenate, diethylaluminum monochloride, diisobutylaluminum monochloride, sesquiethylaluminum chloride, ethylaluminum dichloride, preferably triethylaluminum and triisobutylaluminum.
[0042] The molar ratio of aluminum in the organic aluminum compound to titanium in the catalyst component is 5-5000:1, preferably 20-500:1.
[0043] According to a third aspect of the present invention, the present invention provides an ethylene polymerization method, which comprises: reacting ethylene or ethylene with α-olefin in the presence of the above-mentioned catalyst.
[0044] The ethylene polymerization reaction of the present invention is carried out in a slurry state, and the solvent can be a straight-chain or branched alkane, such as hexane, heptane, octane, decane or its derivatives.
[0045] The reaction conditions include: the reaction pressure is 0.05-10Mpa, preferably 0.1-5Mpa; the reaction temperature is 30-120°C, preferably 40-90°C. When the temperature is too high, the ethylene molecules are prone to free radical polymerization, and the molecular weight of the prepared polyethylene is not high. When the temperature is too low, the catalyst activity is low or no polymerization occurs; the reaction time is 1.5-10h, preferably 1.5-2.5h.
[0046] The present invention will be further described below with reference to the following examples, but is not limited to these examples.
[0047] In the following examples and comparative examples:
[0048] Catalyst component particle size distribution: measured by Mastersizer 2000 instrument, Malvern, UK;
[0049] Polymer apparent bulk density (BD): measured according to ASTM D1895-96;
[0050] Polymer molecular weight (Mw): viscosity method;
[0051] Polymer sphericity and SPAN value: CAMSIZER particle analyzer;
[0052] Note: When the sphericity is 1, the particles are spherical. The smaller the sphericity, the more irregular the particle shape. The smaller the SPAN value, the more concentrated the particle size distribution.
[0053] Examples 1-6 are used to illustrate the catalyst components and catalysts of the present invention and ethylene polymerization reactions.
[0054] Example 1
[0055] 4.8 g of magnesium chloride, 40 ml of toluene, 3.0 ml of epichlorohydrin, 3.6 ml of tributyl phosphate and 7.6 ml of ethanol were added into a reactor, and the mixture was reacted for 1 hour at a stirring speed of 450 rpm and a temperature of 55°C. 20 ml of hexane was added, the temperature was lowered to -30°C, 40 ml of titanium tetrachloride was slowly added dropwise within 4 hours, the temperature was raised to 80°C within 4 hours, and the temperature was kept constant for 2.0 hours. The mother liquor was filtered out with a filter, and the mixture was washed twice with 120 ml of toluene at 60°C, washed 4 times with an organic solvent hexane, and finally 1000 ml of hexane was added to prepare a catalyst component suspension.
[0056] Ethylene polymerization: A 2-liter polymerization kettle was filled with nitrogen and evacuated alternately three times, 1 liter of n-hexane, 2 mmol of triethylaluminum and 1 ml of catalyst component suspension were added, the temperature was raised to 60°C, ethylene was added to maintain the kettle pressure at 0.7 MPa, and the reaction was carried out at 60°C for 2 hours. The catalyst activity was calculated, and the bulk density and particle size distribution of the polymer were determined.
[0057] Example 2
[0058] 4.8 g of magnesium chloride, 40 ml of toluene, 3.0 ml of epichlorohydrin, 3.6 ml of tributyl phosphate and 7.6 ml of ethanol were added into a reactor, and reacted for 1 hour at a stirring speed of 450 rpm and a temperature of 55°C. The temperature was then lowered to -30°C, 80 ml of hexane and 40 ml of titanium tetrachloride were added within 4 hours, the temperature was raised to 80°C within 4 hours, and the temperature was kept constant for 2.0 hours. The mother liquor was filtered out with a filter, and the mixture was washed twice with 120 ml of toluene at 60°C, washed 4 times with an organic solvent hexane, and finally 1000 ml of hexane was added to prepare a catalyst component suspension.
[0059] Ethylene polymerization: Same as Example 1.
[0060] Example 3
[0061] The preparation of the catalyst component is different from that of Example 1 in that titanium tetrachloride is added dropwise after cooling to -10°C.
[0062] Ethylene polymerization: Same as Example 1.
[0063] Example 4
[0064] The preparation of the catalyst component is different from that of Example 1 in that titanium tetrachloride is added dropwise after the temperature is lowered to 20°C.
[0065] Ethylene polymerization: Same as Example 1.
[0066] Example 5
[0067] The preparation of the catalyst component differs from that of Example 1 in that 28 ml of decane is added instead of 20 ml of hexane.
[0068] Ethylene polymerization: Same as Example 1.
[0069] Example 6
[0070] The preparation of the catalyst component differs from that of Example 1 in that 55 ml of hexane is added instead of 20 ml of hexane.
[0071] Ethylene polymerization: Same as Example 1.
[0072] Comparative Example 1
[0073] 4.8 g of magnesium chloride, 55 ml of toluene, 3.0 ml of epichlorohydrin, 3.6 ml of tributyl phosphate and 7.6 ml of ethanol were added into a reactor, and the reaction was carried out for 1 hour at a stirring speed of 450 rpm and a temperature of 55°C. 0.8 g of phthalic anhydride was added, and the temperature was kept constant at 55°C for 1 hour, then the temperature was lowered to -30°C, 40 ml of titanium tetrachloride was added dropwise, and the temperature was raised to 80°C within 4 hours, and the temperature was kept constant for 1.0 hour. The mother liquor was filtered out with a filter, and the catalyst component was washed twice with 120 ml of toluene at 60°C, washed 4 times with an organic solvent hexane, and dried to obtain a catalyst component.
[0074] Ethylene polymerization: Same as Example 1, except that the amount of catalyst component added was 10 mg.
[0075] Comparative Example 2
[0076] 4.8 g of magnesium chloride, 40 ml of toluene, 3.0 ml of epichlorohydrin, 3.6 ml of tributyl phosphate and 7.6 ml of ethanol were added into a reactor, and the mixture was reacted for 1 hour at a stirring speed of 450 rpm and a temperature of 55°C. The mixture was cooled to -30°C, 40 ml of titanium tetrachloride was slowly added dropwise within 4 hours, the mixture was heated to 80°C within 4 hours, and the temperature was kept constant for 2.0 hours. The mother liquor was filtered out with a filter, and the mixture was washed twice with 120 ml of toluene at 60°C, washed 4 times with an organic solvent hexane, and finally 1000 ml of hexane was added to prepare a catalyst component suspension.
[0077] Ethylene polymerization: Same as Example 1.
[0078] Comparative Example 3
[0079] 4.8 g of magnesium chloride, 40 ml of toluene, 3.0 ml of epichlorohydrin, 3.6 ml of tributyl phosphate and 7.6 ml of ethanol were added into a reactor, and reacted for 1 hour at a stirring speed of 450 rpm and a temperature of 55°C. The temperature was then lowered to -30°C, 40 ml of titanium tetrachloride was added within 4 hours, the temperature was raised to 80°C within 4 hours, and the temperature was kept constant for 2.0 hours. The mother liquor was filtered out with a filter, and the mixture was washed twice with 120 ml of toluene at 60°C, washed 4 times with an organic solvent hexane, and finally 1000 ml of hexane was added to prepare a catalyst component suspension.
[0080] Ethylene polymerization: Same as Example 1.
[0081] The catalyst activities and polymer properties of the examples and comparative examples are shown in Table 1.
[0082] Table 1
[0083]
[0084] From the data in Table 1, it can be seen that the activity of the catalyst component of the present invention is significantly higher, the bulk density of the polymer is higher, the sphericity of the polymer is higher, the particle size distribution of the polymer is concentrated, and the particle shape and particle size distribution of the polymer are better.
[0085] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A catalyst component for ethylene polymerization, characterized in that The preparation method of the catalyst component comprises: 1) Mixing a magnesium compound, an organic epoxy compound, an organic phosphorus compound, an organic alcohol compound and a polar diluent, stirring and reacting to obtain a uniform solution; 2) adding a non-polar solvent to a uniform solution at 30-60°C, then cooling to -30°C, adding a titanium compound for contact reaction, heating to precipitate solid particles, washing to obtain a catalyst component or making it into a suspension; the non-polar solvent is hexane; Based on each mole of magnesium compound, the amount of the organic epoxy compound is 0.01-10 moles; the amount of the organic phosphorus compound is 0.01-10 moles; the amount of the organic alcohol compound is 0.01-15 moles; the amount of the polar diluent is 0.2-5L; the amount of the non-polar solvent is 0.2-0.3967125L; and the amount of the titanium compound is 0.2-30 moles.
2. The catalyst component for ethylene polymerization according to claim 1, wherein The magnesium compound is magnesium dihalide or a derivative in which a halogen atom in the molecular formula of magnesium dihalide is replaced by a hydrocarbon group or a halohydrocarbonoxy group.
3. The catalyst component for ethylene polymerization according to claim 1, wherein The organic epoxy compound is at least one of ethylene oxide, propylene oxide, butylene oxide, butadiene oxide, butadiene dioxide, epichlorohydrin, methyl glycidyl ether and diglycidyl ether.
4. The catalyst component for ethylene polymerization according to claim 1, wherein The organic phosphorus compound is selected from the group consisting of hydrocarbon esters or halogenated hydrocarbon esters of orthophosphoric acid, hydrocarbon esters or halogenated hydrocarbon esters of phosphorous acid; The organic alcohol compound is selected from linear alcohols or isomeric alcohols having 1 to 8 carbon atoms.
5. The catalyst component for ethylene polymerization according to claim 4, wherein The organic phosphorus compound is at least one of trimethyl orthophosphate, triethyl orthophosphate, tributyl orthophosphate, triphenyl orthophosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite.
6. The catalyst component for ethylene polymerization according to claim 4, wherein The organic alcohol compound is at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-octanol and isooctanol.
7. The catalyst component for ethylene polymerization according to claim 1, wherein The polar diluent is benzene, toluene, xylene or chlorobenzene.
8. The catalyst component for ethylene polymerization according to claim 1, wherein The general formula of the titanium compound is Ti(OR) a X b , where R is C1-C 14 An aliphatic hydrocarbon group or an aromatic hydrocarbon group, X is a halogen atom, a is an integer from 0 to 2, b is an integer from 0 to 4, and a+b=3 or 4.
9. The catalyst component for ethylene polymerization according to claim 8, wherein The titanium compound is at least one of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium triethoxide monochloride, titanium diethoxide dichloride, titanium trichloride monoethoxide and titanium trichloride.
10. The catalyst component for ethylene polymerization according to claim 9, wherein The titanium compound is titanium tetrachloride, trichloroethoxytitanium or titanium trichloride.
11. The catalyst component for ethylene polymerization according to claim 1, wherein Based on each mole of magnesium compound, the amount of the organic epoxy compound is 0.02-4 moles; the amount of the organic phosphorus compound is 0.02-4 moles; the amount of the organic alcohol compound is 0.05-10 moles; and the amount of the titanium compound is 1-20 moles.
12. The catalyst component for ethylene polymerization according to claim 1, wherein In step 1), the stirring speed is 350-500 rpm, the reaction temperature is 50-100°C, and the reaction time is 0.5-1.5h; In step 2), the heating temperature is 60-110°C.
13. A catalyst for ethylene polymerization, characterized in that The catalyst comprises the catalyst component according to any one of claims 1 to 12, and an organic aluminum compound; The molar ratio of aluminum in the organic aluminum compound to titanium in the catalyst component is 5-5000:
1.
14. The catalyst for ethylene polymerization according to claim 13, wherein The general formula of the organoaluminum compound is AlR 1 n X 3-n , where R 1 is hydrogen, an alkyl group, aralkyl group or aryl group having 1 to 20 carbon atoms; X is chlorine or bromine; and n is a number where 0 < n ≤ 3.
15. The catalyst for ethylene polymerization according to claim 14, wherein The organoaluminum compound is trimethylaluminum, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum monohydrogenate, diisobutylaluminum monohydrogenate, diethylaluminum monochloride, diisobutylaluminum monochloride, sesquiethylaluminum chloride, and ethylaluminum dichloride.
16. The catalyst for ethylene polymerization according to claim 15, wherein The organic aluminum compound is triethylaluminum or triisobutylaluminum.
17. The catalyst for ethylene polymerization according to claim 16, wherein The molar ratio of aluminum in the organic aluminum compound to titanium in the catalyst component is 20-500:
1.
18. An ethylene polymerization method, characterized in that: The ethylene polymerization method comprises: reacting ethylene or ethylene with an α-olefin in the presence of the catalyst described in any one of claims 13 to 17; The reaction conditions include: the reaction pressure is 0.05-10Mpa; the reaction temperature is 30-120°C; and the reaction time is 1.5-10h.
19. The ethylene polymerization process according to claim 18, wherein: The reaction conditions include: the reaction pressure is 0.1-5Mpa; the reaction temperature is 40-90°C; and the reaction time is 1.5-2.5h.