Polyurethane adhesive combined polyether for melamine board, preparation method and application

By using solvent-free polyurethane adhesive combined with polyether on melamine boards, the problem of insufficient adhesive strength and mismatch of drying time is solved, and efficient and environmentally friendly bonding effect is achieved, which is suitable for furniture manufacturing.

CN115975147BActive Publication Date: 2024-11-12SHIJIAZHUANG CHANGHONG BUILDING DECORATION ENG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310130188.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-17
Publication Date
2024-11-12
Estimated Expiration
2043-02-17

AI Technical Summary

Technical Problem

The adhesives of existing melamine boards have problems such as insufficient adhesive strength, long or too short drying time, and poor environmental protection performance, which affects furniture production efficiency and environmental protection requirements.

Method used

A solvent-free polyurethane adhesive combined with melamine plates was developed. By using polyether polyols A and B of different molecular weights and hydroxyl values, combining organic metal catalysts and amine catalysts, the construction time and drying time are adjusted, and the construction time and drying time are increased. Adhesive strength and improve environmental protection performance.

Benefits of technology

It realizes efficient bonding of melamine plates, with construction time greater than 2 hours, curing and drying time less than 24 hours, and is solvent-free, has good environmental protection performance, and is suitable for furniture manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004083512030000021
    Figure BDA0004083512030000021
  • Figure BDA0004083512030000022
    Figure BDA0004083512030000022
  • Figure BDA0004083512030000031
    Figure BDA0004083512030000031
Patent Text Reader

Abstract

The present invention provides a polyurethane adhesive combination polyether for melamine boards, a preparation method and an application, and belongs to the technical field of adhesives. The polyurethane adhesive combination polyether for melamine boards described in the present invention uses polyether polyol A and polyether polyol B with different hydroxyl values ​​and molecular weights, and uses an organic metal catalyst and / or an amine catalyst with a delayed catalytic effect, and accurately controls the amount of catalyst added to ensure sufficient construction time and a shorter curing and drying time. The construction time of the polyurethane adhesive prepared by the combination polyether of the present invention is greater than 2 hours, and the curing and drying time is less than 24 hours, which is particularly suitable for the construction of melamine board bonding. And the polyurethane adhesive prepared using the combination polyether of the present invention has high bonding strength for melamine boards, is solvent-free, and has good environmental performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a polyurethane adhesive for melamine boards. Background Art

[0002] Melamine board, also known as melamine impregnated paper facing board, is a kind of decorative board made by hot pressing after soaking paper with different colors or textures in melamine resin adhesive, drying it to a certain degree of solidification, and then laying it on the surface of particleboard, moisture-proof board, medium-density fiberboard, plywood, blockboard, multilayer board or other hard fiberboard. It has the advantages of flat surface, same expansion coefficient on both sides of the board and not easy to deform, bright color, wear-resistant and corrosion-resistant surface, and economical price, etc. It is widely used in various indoor architectural decorations and the manufacture of various furniture and cabinets.

[0003] When using melamine boards to make furniture or interior decoration, it is inevitable to bond the boards. Currently, there is no special adhesive for melamine boards on the market. Decoration companies or furniture manufacturers mainly use general white latex or polyurethane adhesives for bonding. Since white latex has poor adhesion to melamine boards and is easy to fall off during use, polyurethane adhesives are currently more commonly used.

[0004] Polyurethane adhesives are mostly solvent-based adhesives and water-based adhesives. However, solvent-based adhesives usually contain organic solvents, and their volatilization has a great impact on the environment. Although water-based adhesives are more environmentally friendly, water as a solvent evaporates slowly, and the drying time of adhesives is usually very slow, which affects the production efficiency of furniture manufacturers.

[0005] Moreover, to achieve a good bonding effect on melamine sheets, it is required to reserve appropriate construction time and the shortest possible curing and drying time. However, the general-purpose polyurethane adhesives currently used have the problem of mismatching construction time and drying time. The construction time of water-based polyurethane adhesives is appropriate, greater than or equal to 2 hours, but the curing and drying is relatively slow, often requiring 5 to 7 days; the curing and drying time of solvent-based polyurethane adhesives is appropriate, less than or equal to 24 hours, but the reserved construction time is too short, often less than 30 minutes. In addition, most of the polyurethane adhesives currently used are solvent-based adhesives, which have poor environmental performance and are not conducive to use in the home improvement industry. Summary of the invention

[0006] In view of the above-mentioned defects or deficiencies in the prior art, the present application aims to provide a solvent-free polyurethane adhesive combination polyether for melamine board, a preparation method and application, so as to solve at least one of the above-mentioned technical problems.

[0007] One of the purposes of the present invention is to provide a polyurethane adhesive combination polyether for melamine board, comprising the following raw materials in parts by weight:

[0008]

[0009] The molecular weight of the polyether polyol A is 300-500, and the hydroxyl value is 270-290 mgKOH / g; the molecular weight of the polyether polyol B is 2000-3500, and the hydroxyl value is 55-60 mgKOH / g; and the catalyst includes an organic metal catalyst and / or an amine catalyst.

[0010] Preferably, the composite polyether comprises the following raw materials in parts by weight:

[0011]

[0012]

[0013] Preferably, the mass ratio of the polyether polyol A to the polyether polyol B is 1:1.6-2.5.

[0014] Preferably, the polyether polyol A comprises polyoxypropylene diol, and the polyether polyol B comprises polyoxypropylene triol.

[0015] Preferably, the anti-settling agent includes one or more of organic bentonite, fumed silica, modified castor oil, N-methylpyrrolidone solution of modified polyurea, titanate coupling agent or polyamide wax, preferably N-methylpyrrolidone solution of modified polyurea, and more preferably BYK-410.

[0016] Preferably, the heavy calcium carbonate is 800 mesh heavy calcium carbonate.

[0017] Preferably, the desiccant comprises calcium oxide and / or molecular sieve.

[0018] Preferably, the molecular sieve activation powder includes one or more of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve or 13X molecular sieve, preferably 13X molecular sieve.

[0019] Preferably, the defoaming agent includes a silicone defoaming agent, preferably a polyether-modified silicone defoaming agent.

[0020] Preferably, the nano filler includes one or more of nano calcium carbonate, organic bentonite or kaolin, preferably nano calcium carbonate, and more preferably nano calcium carbonate with a particle size of 0.1 nm to 100 nm.

[0021] Preferably, the chain extender includes one or more of diols or polyols, preferably one or more of 1,2-propylene glycol, glycerol, trimethylolpropane, ethylene glycol or diethylene glycol, more preferably diethylene glycol.

[0022] The second object of the present invention is to provide a method for preparing a polyurethane adhesive combined with polyether for melamine board, the preparation method comprising mixing the components.

[0023] Preferably, polyether polyol A, polyether polyol B, anti-settling agent, moisture absorbent, catalyst, chain extender and defoamer are firstly mixed, and then nano calcium carbonate and filler are added, and then preliminarily mixed and then further mixed.

[0024] Preferably, the catalyst is added by a mother liquor preparation method, including first dissolving the catalyst in polyether polyol A to prepare a catalyst mother liquor with a catalyst content of 1%, and then directly adding the catalyst mother liquor to the composite polyether.

[0025] Preferably, the preparation method further comprises degassing after mixing all the components.

[0026] The third object of the present invention is to provide an application of a polyurethane adhesive combined with polyether for melamine board, comprising: preparing a polyurethane adhesive by mixing the combined polyether with 5 to 20 parts by weight of a polyisocyanate.

[0027] Preferably, the polyisocyanate comprises polymethylene polyphenyl polyisocyanate and / or polymethyl polyphenyl isocyanate.

[0028] The beneficial effects of the present invention include:

[0029] The combined polyether of the present invention uses polyether polyol A and polyether polyol B with different hydroxyl values ​​and molecular weights, and the construction time and drying time when the polyurethane adhesive is prepared using the combined polyether of the present invention are adjusted by reasonably adjusting the ratio of the polyols with different hydroxyl values. The present invention uses an organic metal catalyst and / or an amine catalyst with delayed catalytic effect, and accurately controls the amount of catalyst added to ensure sufficient construction time and a shorter curing and drying time. The construction time of the polyurethane adhesive prepared by the combined polyether of the present invention is greater than 2 hours, and the curing and drying time is less than 24 hours, which is particularly suitable for the construction of melamine board bonding. In addition, the polyurethane adhesive prepared using the combined polyether of the present invention has high bonding strength for melamine boards, is solvent-free, and has good environmental performance. DETAILED DESCRIPTION

[0030] In the following description, certain specific details are included to provide a comprehensive understanding of each disclosed embodiment. However, one skilled in the relevant art will recognize that the embodiments can be implemented without one or more of these specific details, but with other methods, components, materials, etc.

[0031] Unless otherwise required in this application, throughout the specification and the claims that follow, the words "including" and "comprising" should be interpreted in an open, inclusive sense, ie, "including, but not limited to."

[0032] References to "one embodiment" or "an embodiment" or "a preferred embodiment" or "certain embodiments" throughout this specification mean that the specific referenced elements, structures or features described in connection with the embodiment are included in at least one embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" or "in a preferred embodiment" or "in certain embodiments" appearing in different places throughout the specification do not necessarily all refer to the same embodiment. In addition, the specific elements, structures or features may be combined in any appropriate manner in one or more embodiments.

[0033] According to the first aspect of the present invention, a polyurethane adhesive combination polyether for melamine board is provided, comprising the following raw materials in parts by weight:

[0034]

[0035] The number average molecular weight of the polyether polyol A is 400, and the hydroxyl value is 270-290 mgKOH / g; the number average molecular weight of the polyether polyol B is 3000, and the hydroxyl value is 55-60 mgKOH / g; and the catalyst includes an organic metal catalyst and / or an amine catalyst.

[0036] In the present invention, polyether polyol A and polyether polyol B with different hydroxyl values ​​and molecular weights are used to adjust the reaction rate. Low molecular weight polyether polyol A is conducive to improving shear strength, but due to its high hydroxyl value, it reacts too quickly with isocyanate, and the high hydroxyl value will also increase the crosslinking degree of the polyurethane adhesive, thereby increasing the brittleness of the cured polyurethane adhesive and making it easy to break. High molecular weight polyether polyol B, due to its low hydroxyl value, reacts slowly with isocyanate. In addition, introducing polyether polyol B into the polyurethane adhesive can enhance the toughness of the polyurethane adhesive. Therefore, the present invention uses polyether polyol A and polyether polyol B at the same time, and controls the addition amount of polyether polyol A and polyether polyol B to ensure the construction time and curing and drying. The shear strength and toughness of the cured polyurethane adhesive can also be improved.

[0037] In the present invention, the polyether polyol A is, for example, 15 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts or 25 parts. The polyether polyol B is, for example, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts or 35 parts.

[0038] The number average molecular weight of the polyether polyol A is, for example, 300, 320, 340, 360, 380, 400, 420, 440, 460, 480 or 500, and the hydroxyl value is, for example, 270 mgKOH / g, 272 mgKOH / g, 274 mgKOH / g, 276 mgKOH / g, 278 mgKOH / g, 280 mgKOH / g, 282 mgKOH / g, 284 mgKOH / g, 286 mgKOH / g, 288 mgKOH / g. The number average molecular weight of the polyether polyol B is, for example, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400 or 3500, and the hydroxyl value is, for example, 55 mgKOH / g, 56 mgKOH / g, 57 mgKOH / g, 58 mgKOH / g, 59 mgKOH / g or 60 mgKOH / g.

[0039] The present invention uses an organic metal catalyst and / or an amine catalyst, such as an organic metal catalyst, an amine catalyst, or an organic metal and amine catalyst. In the present invention, the organic metal catalyst and the amine catalyst have low catalytic activity in the early stage of the reaction, which can play a delayed catalytic role in the early stage of the reaction, improve the fluidity of the polyurethane adhesive, and thus ensure sufficient construction time; the organic metal catalyst and the amine catalyst have increased catalytic activity in the late stage of the reaction, so they can accelerate the curing and drying time of the polyurethane adhesive in the late stage of the reaction.

[0040] In the present invention, the amount of catalyst used is 0.1 to 0.5 ppm, which means that the amount of catalyst used is 0.1 to 0.5 ppm of the total mass of the combined polyether.

[0041] When the amount of the catalyst is less than 0.1ppm, the catalytic activity is insufficient in the later stage of the reaction, and the required curing and drying time is too long; when the amount of the catalyst is greater than 0.5ppm, the catalytic activity is too high in the early stage of the reaction, and the viscosity of the polyurethane adhesive increases too quickly, and sufficient construction time cannot be guaranteed. Therefore, in the present invention, the amount of the catalyst is 0.1 to 0.5ppm of the total mass of the combined polyether, for example, 0.1ppm, 0.15ppm, 0.2ppm, 0.25ppm, 0.3ppm, 0.35ppm, 0.4ppm, 0.45ppm or 0.5ppm.

[0042] In the present invention, the use of heavy calcium carbonate can effectively reduce costs and adjust density. Heavy calcium carbonate as a filler can increase the product volume of the polyurethane adhesive, thereby reducing costs; it can also adjust the viscosity and rheological properties of the polyurethane adhesive, thereby improving operability during construction; it can also improve the dimensional stability of the polyurethane adhesive after curing, and can also play a reinforcing role for the polyurethane adhesive. In the present invention, the heavy calcium carbonate is, for example, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts or 38 parts.

[0043] In the present invention, the anti-settling agent is mainly used to prevent the filler from settling and causing the oil-powder separation and filler agglomeration. In the present invention, the anti-settling agent is, for example, 0.5 part, 0.55 part, 0.6 part, 0.65 part, 0.7 part, 0.75 part, 0.8 part, 0.85 part, 0.9 part, 0.95 part or 1 part.

[0044] In the present invention, the desiccant is used to absorb water in the combined polyether system to prevent the combined polyether from reacting with water to generate carbon dioxide to form bubbles during the preparation of the polyurethane adhesive by mixing the combined polyether with isocyanate, thereby affecting the shear strength of the polyurethane adhesive after curing and drying. When the amount of the desiccant is less than 2 parts, the water absorption effect is poor and there are many bubbles in the polyurethane adhesive; when the amount of the desiccant is greater than 5 parts, the mechanical properties of the polyurethane adhesive will be affected. Therefore, the desiccant is 2 to 5 parts, for example, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts.

[0045] In the present invention, the defoamer is used to remove bubbles in the polyurethane adhesive system to improve the shear strength of the polyurethane adhesive. The defoamer is, for example, 0.1 part, 0.11 part, 0.12 part, 0.13 part, 0.14 part, 0.15 part, 0.16 part, 0.17 part, 0.18 part, 0.19 part or 0.2 part.

[0046] In the present invention, the nanofiller can increase the shear strength of the polyurethane adhesive after curing and drying. The nanofiller has a small particle size and a large specific surface area, and its addition can make the internal structure of the adhesive more compact after drying.

[0047] In the present invention, the chain extender can extend the polyurethane molecular chain, increase the molecular weight, connect multiple cross-linked polyurethane molecules, form a network interpenetrating structure, shorten the distance between the urethane bonds, increase the intermolecular cohesion of the polyurethane adhesive, and increase the cross-linking points of the adhesive curing reaction, thereby increasing the shear strength of the adhesive. When the chain extender is less than 0.2 parts, the shear strength of the adhesive does not increase significantly; when the chain extender is greater than 0.3 parts, the viscosity of the polyurethane adhesive increases too fast in the early stage, resulting in insufficient operating time. The chain extender is, for example, 0.2 parts, 0.21 parts, 0.22 parts, 0.23 parts, 0.24 parts, 0.25 parts, 0.26 parts, 0.27 parts, 0.28 parts, 0.29 parts or 0.3 parts.

[0048] In a preferred embodiment of the present invention, the composite polyether comprises the following raw materials in parts by weight:

[0049]

[0050]

[0051] In a preferred embodiment of the present invention, the mass ratio of the polyether polyol A to the polyether polyol B is 1:1 to 2.5;

[0052] Preferably, the polyether polyol A comprises polyoxypropylene diol, and the polyether polyol B comprises polyoxypropylene triol.

[0053] In a preferred embodiment of the present invention, the anti-settling agent includes one or more of organic bentonite, fumed silica, modified castor oil, N-methylpyrrolidone solution of modified polyurea, titanate coupling agent or polyamide wax, preferably N-methylpyrrolidone solution of modified polyurea, and more preferably BYK-410.

[0054] In the present invention, the anti-settling agent can form a network structure through hydrogen bonds. After the external shear force is removed, the hydrogen bonds are gradually restored at an appropriate speed, which can slow down the shear recovery speed of the polyurethane adhesive during the construction process. While improving the anti-settling performance of the filler, it can also reduce the viscosity after mixing and improve fluidity, thereby further extending the construction time of the polyurethane adhesive.

[0055] In the present invention, the precipitant is, for example, organic bentonite, fumed silica, modified castor oil, N-methyl pyrrolidone solution of modified polyurea, titanate coupling agent, polyamide wax, N-methyl pyrrolidone solution of modified polyurea and organic bentonite, N-methyl pyrrolidone solution of modified polyurea and fumed silica, N-methyl pyrrolidone solution of modified polyurea and modified castor oil, or a combination of modified castor oil and polyamide wax.

[0056] In a preferred embodiment of the present invention, the heavy calcium carbonate is 800 mesh heavy calcium carbonate.

[0057] In the present invention, the adhesive prepared by using the combined polyether of 800 mesh heavy calcium carbonate has good thixotropy and mechanical properties.

[0058] In a preferred embodiment of the present invention, the moisture absorbent comprises calcium oxide and / or molecular sieve activation powder;

[0059] Preferably, the molecular sieve activation powder includes one or more of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve or 13X molecular sieve, preferably 13X molecular sieve.

[0060] In the present invention, calcium oxide and molecular sieve activation powder can absorb not only water in the polyether system, but also carbon dioxide generated by the reaction of water in the system with isocyanate. The desiccant is, for example, calcium oxide, 3A molecular sieve, 4A molecular sieve, 5A molecular sieve, 13X molecular sieve, calcium oxide and 3A molecular sieve, calcium oxide and 4A molecular sieve, calcium oxide and 5A molecular sieve, calcium oxide and 13X molecular sieve, 13X molecular sieve and 4A molecular sieve, 13X molecular sieve, 4A molecular sieve and 3A molecular sieve, or a combination of 13X molecular sieve, calcium oxide and 5A molecular sieve.

[0061] Preferably, the defoaming agent includes a silicone defoaming agent, preferably a polyether-modified silicone defoaming agent.

[0062] In the present invention, the defoamer is used to remove bubbles in the polyurethane adhesive system to prevent the bubbles in the system from affecting the shear strength of the polyurethane adhesive. The defoamer is, for example, 0.1 part, 0.11 part, 0.12 part, 0.13 part, 0.14 part, 0.15 part, 0.16 part, 0.17 part, 0.18 part, 0.19 part or 0.2 part.

[0063] In a preferred embodiment of the present invention, the nano filler includes one or more of nano calcium carbonate, organic bentonite or kaolin, preferably nano calcium carbonate, and more preferably nano calcium carbonate with a particle size of 0.1 nm to 100 nm.

[0064] In the present invention, the nano filler is, for example, nano calcium carbonate, organic bentonite, kaolin, nano calcium carbonate and organic bentonite, nano calcium carbonate and kaolin, organic bentonite and kaolin, and a combination of nano calcium carbonate, organic bentonite and kaolin.

[0065] The particle size of nano calcium carbonate is, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.

[0066] In the present invention, the surface of the nano calcium carbonate is modified with organic functional groups, which increases the compatibility of the inorganic component and the organic component, thereby improving the shear strength of the adhesive.

[0067] In a preferred embodiment of the present invention, the chain extender includes one or more of diols or polyols, preferably one or more of 1,2-propylene glycol, glycerol, trimethylolpropane, ethylene glycol or diethylene glycol, and more preferably diethylene glycol.

[0068] In the present invention, the chain extender is, for example, 1,2-propylene glycol, glycerol, trimethylolpropane, ethylene glycol, diethylene glycol, a combination of diethylene glycol and 1,2-propylene glycol, a combination of diethylene glycol and glycerol, a combination of diethylene glycol and ethylene glycol, a combination of diethylene glycol, 1,2-propylene glycol and glycerol, a combination of 1,2-propylene glycol, glycerol and trimethylolpropane, or a combination of diethylene glycol, glycerol, trimethylolpropane and ethylene glycol.

[0069] According to a second aspect of the present invention, a method for preparing a polyurethane adhesive combination polyether for melamine boards is provided, the preparation method comprising mixing the components.

[0070] In a preferred embodiment of the present invention, polyether polyol A, polyether polyol B, anti-settling agent, moisture absorbent, catalyst, chain extender and defoamer are first mixed, and then nano calcium carbonate and filler are added, and preliminary mixing is performed first, and then further mixing is performed.

[0071] Specifically, when polyol A, polyol B, anti-settling agent, moisture absorbent, catalyst, chain extender and defoamer are mixed, the rotation speed is 100-200 r / min and the mixing time is 2-3 min; when nano calcium carbonate and filler are added for preliminary mixing, the rotation speed is 400-500 r / min and the mixing time is 5-8 min; when further mixing, the rotation speed is 900-1000 r / min and the mixing time is 10-15 min.

[0072] In a preferred embodiment of the present invention, since the amount of catalyst added is very small, and in the present invention, the amount of catalyst used needs to be accurately controlled, the catalyst is added by a mother liquor preparation method, including first dissolving the catalyst in polyether polyol A to prepare a catalyst mother liquor with a catalyst content of 1%, and then directly using the catalyst mother liquor to add it to the combined polyether.

[0073] In a preferred embodiment of the present invention, the preparation method further comprises degassing after mixing all the components.

[0074] According to a second aspect of the present invention, there is provided an application of a polyurethane adhesive combined with polyether for melamine board, the application comprising: preparing a polyurethane adhesive by mixing the combined polyether with 5 to 20 parts by weight of a polyisocyanate.

[0075] In the present invention, the polyisocyanate is, for example, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.

[0076] In a preferred embodiment of the present invention, the polyisocyanate comprises polymethylene polyphenyl polyisocyanate and / or polymethyl polyphenyl isocyanate.

[0077] In the present invention, the polyisocyanate is, for example, polyisocyanate, polymethyl polyphenyl isocyanate, or a combination of polyisocyanate and polymethyl polyphenyl isocyanate.

[0078] Example

[0079] The present invention is further described in detail below in conjunction with the embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.

[0080] In the following examples, unless otherwise specified, all raw materials are commercially available products.

[0081] raw material

[0082] Polyether polyol A: D204;

[0083] Polyether polyol B: 3050D;

[0084] Polyether polyol C: castor oil modified polyether polyol, THCM-523, number average molecular weight 1000-1500, hydroxyl value 195-205 mgKOH / g;

[0085] Polyether polyol D: tetrahydrofuran modified polyether polyol, PTMG 3000, number average molecular weight 2800-3200, hydroxyl value 35-40 mgKOH / g;

[0086] Anti-settling agent: BYK-410;

[0087] Moisture absorbent: 13X molecular sieve;

[0088] Defoamer: BYK-066N;

[0089] Nano filler: nano calcium carbonate;

[0090] Chain extender: diethylene glycol;

[0091] Catalyst: Tin dilaurate dioctanoate;

[0092] Isocyanate: polymethyl polyphenyl isocyanate PM-200.

[0093] The raw material ratios of Examples 1 to 6 and Comparative Examples 1 to 6 are shown in Tables 1 and 2.

[0094] Table 1 Ratios of raw materials in Examples 1 to 8

[0095]

[0096] Table 2 Ratios of raw materials in comparative examples 1 to 8

[0097]

[0098] Preparation method:

[0099] (1) Add polyether polyol A, polyether polyol B, anti-settling agent, moisture absorbent, catalyst, chain extender and defoamer, and mix them using a high-speed stirrer at a mixing speed of 100 to 200 r / min for 2 to 3 min.

[0100] (2) Add nano fillers and heavy calcium carbonate and perform initial mixing at a rotation speed of 400-500 r / min for 5-8 min.

[0101] (3) The speed is increased to 900-1000 r / min for further mixing, and the mixing time is 10-15 min.

[0102] (4) The mixed materials are subjected to vacuum degassing in a vacuum degassing machine with a stirring device, the stirring speed is 10 to 20 r / min, the vacuum degree is -80 to -90 KPa, and the degassing time is 10 to 15 min to obtain a composite polyether.

[0103] (5) The combined polyether and isocyanate are stirred and mixed, and after mixing, they are applied to the position where the melamine board needs to be bonded within the construction time for bonding operation, and then placed at room temperature for curing.

[0104] Performance tests of the embodiments and comparative examples

[0105] Viscosity: Use a rotational viscometer at 25°C, use a 7# rotor, set the speed to 20 rpm, and measure for 1 minute, that is, read the instantaneous viscosity of the resin at 1 minute.

[0106] The viscosity of the combined polyether at 25°C, the viscosity of the combined polyether and isocyanate after mixing for 2 hours, and the time required for the viscosity to reach 100,000 mPa·s were tested respectively. When the viscosity reaches above 100,000 mPa·s, it is no longer suitable for coating construction.

[0107] Shear strength: The shear strength is tested according to the method in GB / T 7124-2008 Determination of tensile shear strength of adhesives (rigid material to rigid material).

[0108] The shear strength of the polyurethane adhesive was tested after curing for 12 hours and 24 hours.

[0109] Total volatile organic compounds: The total volatile organic compound content is measured in accordance with the test method for the limit of harmful substances in bulk adhesives specified in GB / T 18583-2008 Limits of harmful substances in adhesives for indoor decoration and renovation materials.

[0110] The test results of the embodiments and comparative examples are shown in Table 3 and Table 4:

[0111] Table 3 Test results of Examples 1 to 8

[0112]

[0113] Table 4 Test results of comparative examples 1 to 6

[0114]

[0115]

Claims

1. A polyurethane adhesive for melamine board composed of polyether, It is characterized in that The invention comprises the following raw materials in parts by weight: Polyether polyol A 15~25 parts Polyether polyol B25~35 parts Anti-settling agent 0.5~1 part Catalyst 0.1~0.5ppm Heavy calcium carbonate 28~38 parts 2~5 parts of moisture absorbent Defoaming agent 0.1~0.2 parts 1-10 parts of nanofiller, and Chain extender 0.2~0.5 parts; The number average molecular weight of the polyether polyol A is 300-500, and the hydroxyl value is 270-290 mgKOH / g; the number average molecular weight of the polyether polyol B is 2000-3500, and the hydroxyl value is 55-60 mgKOH / g; and the catalyst includes an organic metal catalyst and / or an amine catalyst.

2. The polyurethane adhesive composition polyether for melamine board according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: Polyether polyol A 18~23 parts Polyether polyol B27~32 parts Anti-settling agent 0.5~1 part Catalyst 0.2~0.4ppm Heavy calcium carbonate 28~38 parts 2~5 parts of moisture absorbent Defoaming agent 0.1~0.2 parts 1-10 parts of nanofiller, and Chain extender 0.2~0.5 parts.

3. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The mass ratio of the polyether polyol A to the polyether polyol B is 1:1-2.

5.

4. The polyurethane adhesive composition polyether for melamine board as claimed in claim 3, It is characterized in that The polyether polyol A includes polyoxypropylene diol, and the polyether polyol B includes polyoxypropylene triol.

5. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The anti-settling agent includes one or more of organic bentonite, fumed silica, modified castor oil, N-methylpyrrolidone solution of modified polyurea, titanate coupling agent or polyamide wax.

6. The polyurethane adhesive composition polyether for melamine board as claimed in claim 5, It is characterized in that The anti-settling agent is a solution of modified polyurea in N-methylpyrrolidone.

7. The polyurethane adhesive composition polyether for melamine board according to claim 6, It is characterized in that The anti-settling agent is BYK-410.

8. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The heavy calcium carbonate is 800 mesh heavy calcium carbonate.

9. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The desiccant includes calcium oxide and / or molecular sieve activation powder.

10. The polyurethane adhesive composition polyether for melamine board according to claim 9, It is characterized in that The molecular sieve activation powder includes one or more of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve or 13X molecular sieve.

11. The polyurethane adhesive composition polyether for melamine board according to claim 10, It is characterized in that The molecular sieve activation powder is 13X molecular sieve.

12. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The defoaming agent includes an organosilicon defoaming agent.

13. The polyurethane adhesive composition polyether for melamine board according to claim 12, It is characterized in that The defoamer is a polyether-modified organic silicon defoamer.

14. The polyurethane adhesive combination polyether for melamine board according to claim 1 or 2, It is characterized in that The nano filler includes one or more of nano calcium carbonate, organic bentonite or kaolin.

15. The polyurethane adhesive composition polyether for melamine board according to claim 14, It is characterized in that The nano filler is nano calcium carbonate.

16. The polyurethane adhesive composition polyether for melamine board according to claim 15, It is characterized in that The particle size of the nano calcium carbonate is 0.1nm~100nm.

17. The polyurethane adhesive composition polyether for melamine board according to claim 1 or 2, It is characterized in that The chain extender includes a polyol.

18. The polyurethane adhesive composition polyether for melamine board according to claim 17, It is characterized in that The chain extender includes one or more of 1,2-propylene glycol, glycerol, trimethylolpropane, ethylene glycol or diethylene glycol.

19. The polyurethane adhesive composition polyether for melamine board according to claim 18, It is characterized in that The chain extender is diethylene glycol.

20. The method for preparing the polyurethane adhesive combined with polyether for melamine board according to any one of claims 1 to 19, It is characterized in that The preparation method comprises mixing the components.

21. The preparation method according to claim 20, It is characterized in that Firstly, polyether polyol A, polyether polyol B, anti-settling agent, moisture absorbent, catalyst, chain extender and defoamer are mixed, and then nano filler and heavy calcium carbonate are added, and preliminary mixing is performed first, and then further mixing is performed.

22. The preparation method according to claim 21, It is characterized in that The catalyst is added by a mother liquor preparation method, including first dissolving the catalyst in polyether polyol A to prepare a catalyst mother liquor with a catalyst content of 1%, and then directly adding the catalyst mother liquor to the composite polyether.

23. The preparation method according to claim 21, It is characterized in that The preparation method further comprises degassing after mixing all the components.

24. Application of the polyurethane adhesive combined with polyether for melamine board according to any one of claims 1 to 19, It is characterized in that The combined polyether is mixed with 5 to 20 parts by weight of polyisocyanate to prepare a polyurethane adhesive.

25. Use of the polyurethane adhesive combined with polyether for melamine board according to claim 24, It is characterized in that The polyisocyanate includes polymethylene polyphenyl polyisocyanate.