A crystal material and its preparation method and application

Through the π conjugation construction and aqueous solution method of the new crystal material 2(C3N6H6)·(C3N6H7)·PF6·H2O, the problems of insufficient transmittance and low birefringence of existing birefringent crystals in the ultraviolet band are solved, achieving It has good transmittance and large birefringence in the range of 200nm ~ 2500nm, and is suitable for applications in optical components and polarizing beam splitting prisms.

CN115976647BActive Publication Date: 2024-10-01FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211085722.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-06
Publication Date
2024-10-01
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

Existing birefringent crystals have insufficient transmittance or low birefringence in the ultraviolet band, which limits their application in the optical field. In particular, there are problems with phase transition and growth difficulties in the deep ultraviolet band and high temperature conditions. .

Method used

A new type of crystal material 2(C3N6H6)·(C3N6H7)·PF6·H2O is used to form a large birefringence through the vertical layered arrangement and three-dimensional structure of π conjugated building units, and the crystal material is prepared by an aqueous solution method , adjust pH value and control reaction conditions to obtain high-quality single crystals.

Benefits of technology

This crystal material has good transmittance in the range of 200nm to 2500nm, and shows a large birefringence at 1020nm, with a birefringence of 0.2545 at 1020nm. It is suitable for applications in optical components and polarizing beam splitting prisms. , improved performance and stability in the ultraviolet band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976647B_ABST
    Figure CN115976647B_ABST
Patent Text Reader

Abstract

The present application discloses a crystal material and a preparation method and application thereof, belonging to the field of optical materials. A crystal material, the chemical formula of which is 2(C 3 N 6 H 6 )·(C 3 N 6 H 7 )·PF 6 ·H 2 O; the crystalline material contains a π-conjugated building unit; the π-conjugated building unit is (C 3 N 6 ) 3‑ ; The π-conjugated building units are perpendicular to the c-axis; The π-conjugated building units are arranged in layers. The first principle calculation shows that the crystal has a large birefringence. The birefringence at 1020nm is 0.2545; The birefringent crystal material has good transmittance in a wide spectrum range of 200nm to 2500nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a crystal material and a preparation method and application thereof, belonging to the field of optical materials. Background Art

[0002] When a beam of light strikes a crystal interface, two refracted beams are generated, a phenomenon known as birefringence. Birefringence arises from the anisotropy of the crystal material itself, and crystals capable of this phenomenon are called birefringent crystals. Crystals capable of birefringence can be categorized as uniaxial or biaxial. Crystals with rhombohedral, tetragonal, or hexagonal systems are uniaxial, while those with orthorhombic, monoclinic, and triclinic systems are biaxial. Birefringent crystals have a wide range of applications in optics, such as photolithography, communications, and micromachining.

[0003] Currently commercially available birefringent crystals include rutile, lithium niobate, yttrium vanadate, calcite, silicon dioxide, magnesium fluoride, and α-BaB2O4. Yttrium vanadate is a high-performance crystal, but its UV cutoff is above 400nm, and its transmittance to wavelengths below 400nm is very poor, making it unsuitable for use in the ultraviolet and deep ultraviolet bands. Magnesium fluoride, with its long transmittance range (110nm to 8500nm), is the only birefringent crystal suitable for use in the ultraviolet and deep ultraviolet bands, but its low birefringence severely limits its application. Silicon dioxide is also plagued by its birefringence. α-BaB2O4 crystals have a wide spectral transmittance range (189nm~3500nm), a short ultraviolet cutoff edge, and a large birefringence (0.159@253.7nm), and have important application value in the ultraviolet region. However, the crystal undergoes phase transition at high temperatures and is extremely prone to cracking during growth, making it difficult to obtain large-sized single crystals.

[0004] With the development of science and technology, people's requirements for birefringent crystals are becoming increasingly higher. Finding excellent birefringent crystals is of great significance, both in terms of quality and quantity. Excellent birefringent crystals must be easy to process and grow, have a large birefringence and transmittance, and have stable physical and chemical properties. Therefore, scientific researchers have been constantly exploring and experimenting in recent years, committed to finding excellent birefringent crystal materials and using them in practical applications. Summary of the Invention

[0005] According to one aspect of the present application, a crystalline material is provided. First-principles calculations show that the material exhibits a high birefringence. The birefringence is 0.2545 at 1020 nm. The birefringent crystalline material 2(C3N6H6)·(C3N6H7)·PF6·H2O provided by the present invention exhibits good transmittance over a broad spectrum of 200 nm to 2500 nm.

[0006] A crystalline material, wherein the chemical formula of the crystalline material is 2(C3N6H6)·(C3N6H7)·PF6·H2O;

[0007] The crystalline material contains π-conjugated building units;

[0008] The π conjugated building unit is (C3N6) 3- ;

[0009] The π-conjugated building unit is perpendicular to the c-axis;

[0010] The π-conjugated building units are arranged in layers.

[0011] Optionally, C3N6H6 are connected by intramolecular NH···N hydrogen bonds;

[0012] (PF6) - It is connected with C3N6H6 through intramolecular hydrogen bonds to form a three-dimensional structure.

[0013] The crystal material contains π-conjugated building blocks (C3N6) 3- The π-conjugated building blocks are arranged in layers perpendicular to the c-axis in the crystal structure. This arrangement induces the formation of large conjugated π bonds, resulting in a high birefringence. Melamine molecules are linked to each other through intramolecular NH···N hydrogen bonds, while PF6 and melamine are linked through intramolecular hydrogen bonds to form a three-dimensional structure.

[0014] Optionally, the crystalline material is a single crystal structure.

[0015] Optionally, the crystalline material belongs to the monoclinic system and has a space group of P21 / n.

[0016] Optionally, the unit cell parameters of the crystal material are as follows:

[0017] α=90°, β=103.664°, γ=90°.

[0018] Optionally, the crystal material has a birefringence of 0.240 to 0.260 at 1020 nm according to first principles calculations.

[0019] According to a second aspect of the present application, a method for preparing a crystalline material is provided.

[0020] The method for preparing the above-mentioned crystal material comprises the following steps:

[0021] A mixture containing melamine, a hexafluorophosphate compound, and water is reacted, and the pH value of the solution is adjusted to a weakly acidic state to obtain the crystalline material;

[0022] The molar ratio of the melamine to the hexafluorophosphate compound is 3:1 to 4:1;

[0023] The molar volume ratio of melamine to water is 1 mmol:25 mL to 1 mmol:35 mL.

[0024] Optionally, the molar ratio of the melamine to the hexafluorophosphate compound is independently selected from any value of 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4:1, or any range between two of them.

[0025] Optionally, the molar volume ratio of melamine to water is independently selected from any value among 1 mmol:25 mL, 1 mmol:27 mL, 1 mmol:30 mL, 1 mmol:32 mL, 1 mmol:35 mL, or any range between the two.

[0026] Optionally, the hexafluorophosphate compound is selected from at least one of LiPF6, NaPF6, KPF6, CsPF6, and HPF6.

[0027] Optionally, the reaction conditions are as follows:

[0028] Temperature is 40℃~90℃;

[0029] The time is 30 minutes to 60 minutes.

[0030] Optionally, the reaction temperature is independently selected from any value among 40°C, 42°C, 50°C, 55°C, 60°C, 65°C, 70°C, 80°C, 90°C or any range therebetween.

[0031] Optionally, the reaction time is independently selected from any value among 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, or any range therebetween.

[0032] According to a third aspect of the present application, an application of a crystalline material is provided.

[0033] Application of the above-mentioned crystal material and / or the crystal material obtained by the above-mentioned preparation method in the preparation of polarization beam splitting prisms or optical elements.

[0034] Optionally, the polarization beam splitter prism is selected from one of a Glan prism, a Wollaston prism, a Rochon prism, and a beam splitting polarizer;

[0035] The optical element is selected from one of an optical isolator, a circulator, a beam displacer, an optical polarizer, an optical modulator, an optical polarizer, a polarization beam splitter, a phase delay device, and an electro-optical modulation device.

[0036] The beneficial effects of this application include:

[0037] 1) This application provides a crystal material with a high birefringence, as shown by first-principles calculations. The birefringence is 0.2545 at 1020 nm. The birefringent crystal material 2(C3N6H6)·(C3N6H7)·PF6·H2O provided by the present invention exhibits good transmittance over a broad spectrum of 200 nm to 2500 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the structure of the 2(C3N6H6)·(C3N6H7)·PF6·H2O crystal obtained in Examples 1-3.

[0039] Figure 2 This is the birefringence spectrum of the 2(C3N6H6)·(C3N6H7)·PF6·H2O crystal obtained in Examples 1-3.

[0040] Figure 3 This is a schematic diagram of the polarization beam splitter prism produced in Example 4. DETAILED DESCRIPTION

[0041] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0042] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0043] The analysis method in the examples of this application is as follows:

[0044] The crystal structure data was measured using a Rigaku ROD, Synergy Custom system four-circle diffractometer with a wavelength of Ga Kα radiation. Data collection was performed at room temperature;

[0045] The birefringence data of the crystals were obtained by first-principles calculations using Materials Studio 8.0 software, with all parameters set to default values ​​without further adjustment.

[0046] Example 1

[0047] A method for preparing 2(C3N6H6)·(C3N6H7)·PF6·H2O birefringent crystals by aqueous solution method comprises the following steps:

[0048] 1) Dissolve 3 mmol of melamine and 1 mmol of sodium hexafluorophosphate in a clean beaker containing 35 mL of water and adjust the pH of the solution to a weakly acidic state.

[0049] 2) Heat the mixed aqueous solution to 60°C on a magnetic stirrer and stir continuously for 60 minutes. Then cool and crystallize at room temperature. After three to five days, a large number of colorless, transparent single crystals will appear.

[0050] 3) The crystals obtained in step 2) were washed with purified water and then dried naturally. The sample obtained in Example 1 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and refinement of the data was as follows: Figure 1 shown.

[0051] 4) The single crystal data obtained in step 3) were calculated using first principles calculations, which showed that the compound had a large birefringence of 0.2545 at 1020 nm.

[0052] Example 2

[0053] A method for preparing 2(C3N6H6)·(C3N6H7)·PF6·H2O birefringent crystals by aqueous solution method comprises the following steps:

[0054] 1) Dissolve 3.5 mmol of melamine and 1 mmol of potassium hexafluorophosphate in a clean beaker containing 30 mL of water and adjust the pH of the solution to a weakly acidic state.

[0055] 2) Heat the mixed aqueous solution to 50°C on a magnetic stirrer and stir continuously for 45 minutes. Then cool and crystallize at room temperature. After three to five days, a large number of colorless, transparent single crystals will appear.

[0056] 3) The crystals obtained in step 2) were washed with purified water and then dried naturally. The sample obtained in Example 2 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and refinement of the data was as follows: Figure 1 shown.

[0057] 4) The single crystal data obtained in step 3) were calculated using first principles calculations, which showed that the compound had a large birefringence of 0.2545 at 1020 nm.

[0058] Example 3

[0059] A method for preparing 2(C3N6H6)·(C3N6H7)·PF6·H2O birefringent crystals by aqueous solution method comprises the following steps:

[0060] 1) Dissolve 3 mmol of melamine and 1 mmol of lithium hexafluorophosphate in a clean beaker containing 25 mL of water and adjust the pH of the solution to a weakly acidic state.

[0061] 2) Heat the mixed aqueous solution to 80°C on a magnetic stirrer and stir continuously for 30 minutes. Then cool and crystallize at room temperature. After three to five days, a large number of colorless, transparent single crystals will appear.

[0062] 3) The crystals obtained in step 2) were washed with purified water and then dried naturally. The sample obtained in Example 3 was placed on a four-circle diffractometer to collect diffraction data. The crystal structure obtained after software restoration and refinement of the data was as follows: Figure 1 shown.

[0063] 4) The single crystal data obtained in step 3) were calculated using first principles calculations, which showed that the compound had a large birefringence of 0.2545 at 1020 nm.

[0064] Example 4 Polarizing Prism

[0065] After processing any 2(C3N6H6)·(C3N6H7)·PF6·H2O crystals obtained in Examples 1-3, they are bonded together to make the following Figure 3 Polarizing prism, when the light beam is incident vertically on the prism surface, neither the o-light nor the e-light is deflected in prism 1; the o-light is completely reflected at the glued surface and completely absorbed by the absorption coating on the prism surface, while the e-light is emitted from the second prism.

[0066] The above descriptions are merely a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application discloses the preferred embodiments as above, they are not intended to limit the present application. Any technical personnel familiar with the present profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A crystalline material, characterized in that: The chemical formula of the crystalline material is 2(C3N6H6)·(C3N6H7)·PF6·H2O; The crystalline material contains π-conjugated building units; The π-conjugated building unit is (C3N6) 3- ; The π-conjugated building unit is perpendicular to the c-axis; The π-conjugated building units are arranged in layers; The crystal material belongs to the monoclinic system, and the space group is P twenty one / n ; The unit cell parameters of the crystal material are as follows: a=12.8762(10) Å,b=10.8891(8) Å,c=15.2192(13) Å, α =90°, β =103.664°, γ =90°。 2. The crystal material according to claim 1, characterized in that C3N6H6 are connected by intramolecular N−H···N hydrogen bonds; (PF6) - It is connected with C3N6H6 through intramolecular hydrogen bonds to form a three-dimensional structure.

3. The crystal material according to claim 1, characterized in that The crystal material is a single crystal structure.

4. The crystalline material according to claim 1, characterized in that The crystalline material has a birefringence of 0.240 to 0.260 at 1020 nm according to first principle calculations.

5. The method for preparing the crystalline material according to any one of claims 1 to 4, characterized in that: The following steps are involved: A mixture containing melamine, a hexafluorophosphate compound and water is reacted to obtain the crystalline material by adjusting the pH value of the solution to a weak acidity; The molar ratio of the melamine to the hexafluorophosphate compound is 3:1 to 4:1; The molar volume ratio of melamine to water is 1 mmol:25 mL to 1 mmol:35 mL; The reaction conditions are as follows: Temperature: 40℃ ~ 90℃; The time is 30 min ~ 60 min.

6. The preparation method according to claim 5, characterized in that: The hexafluorophosphate compound is selected from at least one of LiPF6, NaPF6, KPF6, CsPF6, and HPF6.

7. Use of the crystal material according to any one of claims 1 to 4 and / or the crystal material obtained by the preparation method according to any one of claims 5 to 6 in the preparation of a polarization beam splitter prism.

8. The use according to claim 7, characterized in that: The polarization beam splitter prism is selected from one of a Glan prism, a Wollaston prism, a Rochon prism, and a beam splitting polarizer.

9. Use of the crystal material according to any one of claims 1 to 4 and / or the crystal material obtained by the preparation method according to any one of claims 5 to 6 in the preparation of optical elements.

10. The use according to claim 9, characterized in that: The optical element is selected from one of an optical isolator, a circulator, a beam displacer, an optical polarizer, an optical modulator, an optical polarizer, a polarization beam splitter, a phase delay device, and an electro-optical modulation device.