A method for preparing a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst, a catalyst prepared thereby and its use
By using the ZSM-12 molecular sieve catalyst containing Fe, the problem of insufficient selectivity of xylene liquid phase isomerization reaction and complex and high cost in the prior art is solved, and efficient and low-cost catalyst preparation and reaction performance are achieved, simplifying the The catalyst preparation process is carried out.
Patent Information
- Application Number
- CN202111224504.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-19
AI Technical Summary
The existing xylene liquid phase isomerization catalysts have shortcomings in improving reaction selectivity, and require trace amounts of hydrogen to maintain stability, and the preparation process is complex and costly.
Using Fe-containing ZSM-12 molecular sieve as a catalyst, by mixing silicon source, aluminum source, iron source, template agent and water, crystallization, filtering, washing and drying, the Fe-containing ZSM-12 molecular sieve was obtained and inert with the inert. After the support and the gel solvent are formed, ammonium exchange is performed to prepare a non-hydrogen liquid phase alkylaromatic isomerization catalyst.
Achieving high activity and excellent selectivity liquid phase isomerization reaction of large xylene, simplifying the catalyst preparation process, reducing costs, and eliminating the need for additional metal-loading steps, the catalyst exhibits good stability under non-hyaluron conditions. and efficiency.
Smart Images

Figure CN115990517B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of alkyl aromatic hydrocarbon isomerization, and in particular to a method for preparing a non-hydrogenated liquid phase alkyl aromatic hydrocarbon isomerization catalyst, a catalyst prepared thereby and a use thereof. Background Art
[0002] Xylene isomerization is an important component of the aromatics complex. In recent years, the catalytic activity of the xylene isomerization unit has approached the upper limit of thermodynamic equilibrium. The key to further improving quality and efficiency lies in improving the selectivity of the reaction process.
[0003] The reaction mechanism analysis of xylene isomerization shows that both isomerization and disproportionation are reactions catalyzed by B (Bronsted) acid, and the only difference is the required pore space and elementary reaction energy barrier. The disproportionation energy barrier is higher than that of isomerization, so in order to suppress the disproportionation side reaction, a lower reaction temperature should be selected.
[0004] US20110263918 A1 introduces a xylene isomerization process, which uses HZSM-5 or MCM-49 molecular sieves as catalysts for acidic components. Under conditions where the temperature is below 295°C and the pressure ensures that the reactants are liquid, a xylene component close to the equilibrium composition can be obtained. The process can be operated continuously under the condition that the feed only contains ppm-level dissolved hydrogen. It can also be cyclically applied in non-hydrogen-containing feeds, but the catalyst needs to be periodically regenerated with low-ppm-level hydrogen.
[0005] The document "Study on the Catalyst for Liquid-Phase Isomerization of Xylene" (Petrochemical Industry, Vol. 7, No. 3, 1978) studied the performance of the liquid-phase isomerization of xylene over the ZSM-5 catalyst synthesized from water glass, aluminum sulfate, sulfuric acid and ethylamine. The experimental results showed that the ZSM-5 zeolite catalyst has high activity and selectivity for liquid-phase isomerization of xylene and is applicable to mixed xylene feedstocks containing ethylbenzene.
[0006] Although the above-mentioned catalysts of the prior art have high xylene liquid phase isomerization reaction activity, a trace amount of dissolved hydrogen is required to maintain the stability of the catalyst, and when high activity is achieved, the reaction selectivity needs to be improved.
[0007] Therefore, it is necessary to explore new acidic materials for the preparation and modification of liquid-phase alkyl aromatic isomerization catalysts, so that the catalysts have both good alkyl aromatic liquid-phase isomerization reaction activity and excellent reaction selectivity, and at the same time their preparation process is simple, efficient and low-cost. Summary of the invention
[0008] After in-depth research and a large number of experiments, the inventors found that the Fe-containing ZSM-12 molecular sieve has high isomerization activity and para-alkyl aromatics selectivity, low preparation cost, simple and efficient process, and completed the present invention on this basis.
[0009] In one aspect, the present invention provides a method for preparing a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst, the method comprising:
[0010] (1) mixing a silicon source, an aluminum source, an iron source, a template (T) and water into a uniform mixture, and the mixture is crystallized, filtered, washed and dried to obtain a ZSM-12 molecular sieve containing Fe;
[0011] (2) uniformly kneading the Fe-containing ZSM-12 molecular sieve with the inert carrier and the peptizing agent solution and forming the mixture, followed by drying and calcining to obtain a catalyst precursor; and
[0012] (3) exchanging the catalyst precursor with an ammonium salt, and obtaining the non-hydrogen-containing liquid phase alkyl aromatic isomerization catalyst after drying and calcining.
[0013] The present invention also provides a method for preparing a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst, the method comprising:
[0014] (1) mixing a silicon source, an aluminum source, an iron source, a template and water into a uniform mixture, and the mixture is crystallized, filtered, washed and dried to obtain a ZSM-12 molecular sieve containing Fe;
[0015] (2) exchanging the Fe-containing ZSM-12 molecular sieve with an ammonium salt, followed by drying and calcining to obtain a hydrogen-type Fe-containing ZSM-12 molecular sieve; and
[0016] (3) The hydrogen-type Fe-containing ZSM-12 molecular sieve is uniformly kneaded with an inert carrier and a peptizing agent solution and formed, and then dried and calcined to obtain the non-hydrogen-containing liquid phase alkyl aromatic isomerization catalyst.
[0017] In one embodiment of the method according to the present invention, the molar ratio of the silicon source, aluminum source, iron source, template and water is SiO2:Al2O3:Fe2O3:template:H2O=1:(0.005~0.05):(0.005~0.05):(0.05~1):(10~60).
[0018] In another embodiment of the method according to the present invention, the silicon source is water glass, liquid silica sol or solid silica sol; when the silicon source is water glass, the molar ratio of sodium oxide to silicon oxide in the water glass is (0.01-0.4):1; when the silicon source is liquid silica sol, the concentration of the liquid silica sol is 10-40% by mass, preferably 20-40% by mass; when the silicon source is solid silica sol, the particle size of the solid silica sol is 0.005-0.05 μm, preferably 0.01-0.03 μm.
[0019] In another embodiment of the method according to the present invention, the aluminum source is one or more selected from aluminum sulfate, aluminum chloride, aluminum acetate, and aluminum nitrate; the iron source is one or more selected from iron sulfate, iron chloride, and iron nitrate.
[0020] In another embodiment of the method according to the present invention, the template is a material having the general formula N(R)4 + X - A quaternary ammonium salt of, wherein R is an alkyl group having 1 to 4 carbon atoms, preferably an ethyl group or a propyl group; X - is a hydroxide ion or a halogen anion, preferably a bromide ion; and the molar ratio of the template is X - :SiO2=0.05~1.
[0021] In another embodiment of the method according to the present invention, the crystallization temperature in step (1) is 130-190° C., preferably 140-180° C.; the crystallization time is 18-100 hours, preferably 20-96 hours.
[0022] In another embodiment of the method according to the present invention, the inert carrier is aluminum oxide or silicon oxide.
[0023] In another embodiment of the method according to the present invention, the peptizing agent is one or more selected from nitric acid, phosphoric acid, and citric acid, and the concentration of the peptizing agent solution is 1 to 5% by mass.
[0024] In another embodiment of the method according to the present invention, the ammonium salt is ammonium chloride or ammonium nitrate, and its usage concentration is 1 to 30% by mass, preferably 3 to 10% by mass.
[0025] In another embodiment of the method according to the present invention, the drying is independently carried out at a temperature of 100-140°C for 4-24 hours; the calcination after molding is carried out at a temperature of 520-550°C for 2-24 hours; and the calcination after ammonium exchange is carried out at a temperature of 400-500°C for 2-24 hours.
[0026] On the other hand, the present invention provides a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst prepared according to any of the aforementioned methods, the catalyst comprising: 24.0 to 99.9 mass % of Fe-containing ZSM-12 molecular sieve; and 0.1 to 76.0 mass % of an inert carrier.
[0027] In one embodiment of the catalyst according to the present invention, the catalyst comprises 40.0 to 70.0 mass % of a ZSM-12 molecular sieve containing Fe.
[0028] In another embodiment of the catalyst according to the present invention, the silicon-aluminum ratio of the Fe-containing ZSM-12 molecular sieve is 20-200, preferably 30-150; the silicon-iron ratio is 20-200, preferably 40-120.
[0029] In another embodiment of the catalyst according to the present invention, the inert carrier is aluminum oxide or silicon oxide.
[0030] In another aspect, the present invention provides a use of the catalyst according to any of the above embodiments in the isomerization of non-hydrogenated liquid phase alkyl aromatic hydrocarbons, comprising: isomerizing the alkyl aromatic hydrocarbons at 240 to 310° C. and a weight hourly space velocity of 1 to 10 h under a reaction pressure that maintains the alkyl aromatic hydrocarbons in a liquid state. -1 under the conditions of , contacting with the catalyst to carry out isomerization reaction.
[0031] In one embodiment of the use according to the present invention, the alkyl aromatic hydrocarbon is a C8-C10 aromatic hydrocarbon.
[0032] The catalyst is prepared by the method of the present invention, the molecular sieve synthesis is optimized, Fe is directly added during the molecular sieve synthesis, and the subsequent catalyst preparation process does not require additional metal loading steps such as impregnation, thereby simplifying the catalyst preparation process, shortening the preparation cycle, and improving the preparation efficiency.
[0033] The catalyst prepared by the method of the present invention comprises an Fe-containing ZSM-12 molecular sieve acidic activation component, and compared with catalysts comprising other molecular sieve active components, good alkyl aromatic hydrocarbon isomerization activity and selectivity are obtained at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Example 1;
[0035] Figure 2 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Example 2;
[0036] Figure 3 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Example 3;
[0037] Figure 4 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Example 4;
[0038] Figure 5 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Example 5;
[0039] Figure 6 is the XRD spectrum of the ZSM-12 molecular sieve prepared according to Comparative Example 1; and
[0040] Figure 7 The XRD spectrum of the ZSM-12 molecular sieve prepared according to Comparative Example 2. DETAILED DESCRIPTION
[0041] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. Through these descriptions, the features and advantages of the present application will become clearer and more explicit.
[0042] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0043] According to the preparation method of the present invention, during the preparation process, the molecular sieve synthesis is optimized, Fe is directly added during the molecular sieve synthesis process, and the subsequent catalyst preparation process does not require additional metal loading steps such as impregnation, thereby simplifying the catalyst preparation process, shortening the preparation cycle, and improving the preparation efficiency.
[0044] In the synthesis process of Fe-containing molecular sieve ZSM-12, silicon source, aluminum source, iron source, template and water are used. The molar ratio of silicon source, aluminum source, iron source, template and water should meet the following conditions: SiO2:Al2O3:Fe2O3:template:H2O=1:(0.005-0.05):(0.005-0.05):(0.05-1):(10-60), wherein the silicon source can be water glass, liquid silica sol or solid silica sol, the aluminum source is aluminum sulfate, and the iron source is iron sulfate. The molar ratio of sodium oxide to silicon oxide in the water glass is (0.01-0.4):1, the concentration of the liquid silica sol is 10-40% by mass, preferably 20-40% by mass, and the particle size of the solid silica sol is 0.005-0.05 μm, preferably 0.01-0.03 μm. The template used is a catalyst having the general formula N(R)4 + X - R is an alkyl group having 1 to 4 carbon atoms, preferably an ethyl group or a propyl group, and X - is a hydroxide ion or a halogen anion, preferably a bromide ion, N is a nitrogen atom, and the amount of the template agent is in accordance with the molar ratio X - :SiO2=0.05~1.
[0045] The crystallization temperature of the molecular sieve is 130 to 190° C., preferably 140 to 180° C.; the crystallization time is 18 to 100 hours, preferably 20 to 96 hours.
[0046] Specifically, the non-hydrogenated liquid phase alkyl aromatic isomerization catalyst is prepared according to the preparation method of the present invention as follows:
[0047] The Fe-containing ZSM-12 molecular sieve is synthesized to obtain the molecular sieve raw powder, which is washed with deionized water to neutrality with a pH range of 6 to 8. The inert carrier is mixed with the Fe-containing ZSM-12 molecular sieve, a peptizing agent solution is added and kneaded evenly, and then extruded into strips, dried at a temperature of 100 to 140° C. for 4 to 24 hours, and calcined in an air atmosphere at a temperature of 520 to 550° C. for 2 to 24 hours. The obtained shaped carrier is ammonium exchanged with an ammonium salt solution such as ammonium chloride or ammonium nitrate, and the ammonium salt solution concentration is 1 to 30% by mass, preferably 3 to 10% by mass. Then it is dried at a temperature of 100 to 140° C. for 4 to 24 hours, and then calcined in an air atmosphere at a temperature of 400 to 500° C. for 2 to 24 hours to obtain the catalyst.
[0048] Alternatively, as an alternative, the Fe-containing ZSM-12 molecular sieve raw powder can also be ammonium exchanged using an ammonium salt solution such as ammonium chloride or ammonium nitrate, with a concentration of 1 to 30% by mass, preferably 3 to 10% by mass. Then, it is dried at a temperature of 100 to 140°C for 4 to 24 hours, and then calcined at a temperature of 400 to 500°C to obtain a hydrogen-type molecular sieve. The hydrogen-type molecular sieve is mixed with an inert carrier, kneaded and formed, dried at a temperature of 100 to 140°C for 4 to 24 hours, and then calcined at a temperature of 520 to 550°C for 2 to 24 hours to obtain the catalyst.
[0049] According to the preparation method of the present invention as described above, the obtained non-hydrogenated liquid phase alkyl aromatic isomerization catalyst includes a ZSM-12 molecular sieve containing Fe, the content of which can be 24 to 99.9% by mass, preferably 40 to 70% by mass, the silicon-aluminum ratio can be 20 to 200, preferably 30 to 150, and the silicon-iron ratio is 20 to 200, preferably 40 to 120; the remaining components are inert carriers, which can be aluminum oxide or silicon oxide.
[0050] The catalyst prepared by the method of the present invention can be used for the isomerization of non-hydrogenated liquid phase alkyl aromatics, comprising the steps of: isomerizing the alkyl aromatics at 240-310°C and a weight hourly space velocity of 1-10h under a reaction pressure to maintain the liquid state; -1 The catalyst of the present invention is used for isomerization of C8 aromatics to increase the yield of p-xylene and maintain good selectivity.
[0051] The catalyst performance is evaluated according to the following calculation method:
[0052] Isomerization activity index:
[0053] Xylene yield:
[0054] The present invention is described in detail below by way of examples, but the present invention is not limited thereto.
[0055] Philips XPert diffractometer was used to determine the crystal structure of the molecular sieve, Cu Kα radiation, 2θ scanning range 5°~35°, and external standard method for quantification. Rigaku Corporation 3013 X-ray fluorescence spectrometer was used to determine the chemical composition of the sample and calculate the silicon-aluminum ratio of the molecular sieve, tungsten target, excitation voltage 40 kV, and excitation current 50 mA.
[0056] Example
[0057] Example 1
[0058] (1) Preparation of Fe-containing ZSM-12 molecular sieve
[0059] In a 200 mL reactor, 58.5 g of water glass (SiO2 content: 24.01% by mass, Na2O content: 7.08% by mass, Al2O3 content: 0.2% by mass, the same below), 1.83 g of aluminum sulfate 18hydrate Al2(SO4)3·18H2O, 1.59 g of iron sulfate Fe2(SO4)3, 9.84 g of tetraethylammonium bromide N(C2H5)4 + Br - As a template (T), 0.8 g of deionized water was mixed evenly to obtain a mixture to be crystallized; wherein the molar ratio of each material was Na2O:SiO2:Al2O3:Fe2O3:T:H2O=0.28:1:0.017:0.017:0.2:10.
[0060] The mixture to be crystallized was hydrothermally crystallized at 150°C for 60 hours, and the solid obtained after crystallization was washed with excess deionized water until the pH value of the eluate was 6-8, which was neutral, and then dried at 120°C for 6 hours to obtain a ZSM-12 molecular sieve containing Fe, denoted as Z-1, whose silicon oxide / aluminum oxide molar ratio was 60, and whose silicon oxide / iron oxide molar ratio was 65 (determined by XRF method, the same below). The XRD diffraction spectrum of Z-1 is shown in Figure 1 .
[0061] (2) Preparation of Catalyst
[0062] Take the ZSM-12 molecular sieve powder Z-1 prepared in step (1) and mix it with alumina in a mass ratio of 7:3. Add 5% by mass nitric acid aqueous solution and knead it evenly, the nitric acid aqueous solution used accounts for 40% by mass of the solid mixture, and then extrude it into strips. Dry the strips at 120°C for 6 hours, then cut them into pellets and roast them at 540°C for 4 hours. The roasted sample is ion exchanged with 5% by mass ammonium chloride aqueous solution at 90°C for 2 hours, washed until there is no chloride ion in the mother liquor, dried at 120°C for 6 hours, and roasted at 500°C for 4 hours to obtain catalyst C-1.
[0063] Example 2
[0064] (1) Preparation of Fe-containing ZSM-12 molecular sieve
[0065] Molecular sieve Z-2 was synthesized according to the method of Example 1, except that the molar ratio of the materials was Na2O:SiO2:Al2O3:Fe2O3:T:H2O=0.28:1:0.017:0.01:0.2:10. The XRD diffraction spectrum of Z-2 is shown in Figure 2 .
[0066] (2) Preparation of Catalyst
[0067] Catalyst C-2 was obtained according to the preparation method (2) in Example 1.
[0068] Example 3
[0069] (1) Preparation of Fe-containing ZSM-12 molecular sieve
[0070] Molecular sieve Z-3 was synthesized according to the method of Example 1, except that the molar ratio of the materials was Na2O:SiO2:Al2O3:Fe2O3:T:H2O=0.28:1:0.01:0.01:0.2:10. The XRD diffraction spectrum of Z-3 is shown in Figure 3 .
[0071] (2) Preparation of Catalyst
[0072] Catalyst C-3 was obtained according to the preparation method (2) in Example 1.
[0073] Example 4
[0074] (1) Preparation of Fe-containing ZSM-12 molecular sieve
[0075] Molecular sieve Z-4 was synthesized according to the method of Example 1, except that the molar ratio of the materials was Na2O:SiO2:Al2O3:Fe2O3:T:H2O=0.28:1:0.01:0.017:0.2:10. The XRD diffraction spectrum of Z-4 is shown in Figure 4 .
[0076] (2) Preparation of Catalyst
[0077] Catalyst C-4 was obtained according to the preparation method (2) in Example 1.
[0078] Example 5
[0079] (1) Preparation of Fe-containing ZSM-12 molecular sieve
[0080] Molecular sieve Z-5 was synthesized according to the method of Example 1, except that the molar ratio of the materials was Na2O:SiO2:Al2O3:Fe2O3:T:H2O=0.28:1:0.01:0.007:0.3:10. The XRD diffraction spectrum of Z-5 is shown in Figure 5 .
[0081] (2) Preparation of Catalyst
[0082] Catalyst C-5 was obtained according to the preparation method (2) in Example 1.
[0083] Comparative Example 1
[0084] (1) Preparation of Fe-free ZSM-12 molecular sieve
[0085] In a 200 mL reactor, 58.5 g of water glass (SiO2 content: 24.01% by mass, Na2O content: 7.08% by mass, Al2O3 content: 0.2% by mass, the same below), 1.83 g of aluminum sulfate 18 hydrate Al2(SO4)3·18H2O, 9.84 g of tetraethylammonium bromide N(C2H5) were added. 4+ Br - As a template (T), 0.80 g of deionized water was mixed evenly to obtain a mixture to be crystallized; wherein the molar ratio of each material was Na2O:SiO2:Al2O3:T:H2O=0.28:1:0.017:0.2:10.
[0086] The mixture to be crystallized was hydrothermally crystallized at 170°C for 35 hours, and the solid obtained after crystallization was washed with excess deionized water until the pH value of the eluate was 6-8, which was neutral, and then dried at 120°C for 6 hours to obtain a ZSM-12 molecular sieve, denoted as Z-6, with a silicon oxide / aluminum oxide molar ratio of 58 (determined by XRF method, the same below). The XRD diffraction spectrum of Z-6 is shown in Figure 6 .
[0087] (2) Preparation of Catalyst
[0088] Take the ZSM-12 molecular sieve powder Z-6 prepared in step (1) and mix it with alumina in a mass ratio of 7:3. Add 5% by mass nitric acid aqueous solution and knead it evenly, the nitric acid aqueous solution used accounts for 40% of the mass of the solid mixture, and then extrude it into strips. Dry the strips at 120°C for 6 hours, then cut into pellets and calcine at 540°C for 4 hours. The calcined sample is ion exchanged with 5% by mass ammonium chloride aqueous solution at 90°C for 2 hours, washed until there is no chloride ion in the mother liquor, dried at 120°C for 6 hours, and calcined at 500°C for 4 hours to obtain catalyst D-1.
[0089] Comparative Example 2
[0090] (1) Preparation of Fe-free ZSM-12 molecular sieve
[0091] The ZSM-12 molecular sieve Z-7 was prepared according to the method of Comparative Example 1, except that the molar ratio of the materials was Na2O:SiO2:Al2O3:T:H2O=0.28:1:0.01:0.2:10. The molar ratio of silicon oxide to aluminum oxide was 88 (determined by XRF method, the same below). The XRD diffraction spectrum of Z-7 is shown in Figure 7 .
[0092] (2) Preparation of Catalyst
[0093] Catalyst D-2 was obtained according to the preparation method (2) in Comparative Example 1.
[0094] Comparative Example 3
[0095] A ZSM-5 molecular sieve with a silicon-aluminum ratio of 60 was used as the acidic material and was fully mixed with alumina at a mass ratio of 7:3. A nitric acid aqueous solution with a concentration of 5% by mass was added and kneaded evenly, and the nitric acid aqueous solution used accounted for 40% of the mass of the solid mixture, and then extruded into strips. The strips were dried at 120°C for 6 hours, then pelletized and calcined at 540°C for 4 hours. The calcined sample was ion exchanged with an ammonium chloride aqueous solution with a concentration of 5% by mass at 90°C for 2 hours, washed until there was no chloride ion in the mother liquor, dried at 120°C for 6 hours, and calcined at 500°C for 4 hours to obtain catalyst D-3.
[0096] Comparative Example 4
[0097] ZSM-11 molecular sieve with a silicon-aluminum ratio of 60 was used as the acidic material, and was fully mixed with alumina at a mass ratio of 7:3. A nitric acid aqueous solution with a concentration of 5% by mass was added and kneaded evenly, and the nitric acid aqueous solution used accounted for 40% of the mass of the solid mixture, and then extruded into strips. The strips were dried at 120°C for 6 hours, then pelletized and calcined at 540°C for 4 hours. The calcined sample was ion exchanged with an ammonium chloride aqueous solution with a concentration of 5% by mass at 90°C for 2 hours, washed until there was no chloride ion in the mother liquor, dried at 120°C for 6 hours, and calcined at 500°C for 4 hours to obtain catalyst D-4.
[0098] Comparative Example 5
[0099] EU-1 molecular sieve with a silicon-aluminum ratio of 30 was used as the acidic material, and it was fully mixed with alumina at a mass ratio of 7:3. A nitric acid aqueous solution with a concentration of 5% by mass was added and kneaded evenly, and the nitric acid aqueous solution used accounted for 40% of the mass of the solid mixture, and then extruded into strips. The strips were dried at 120°C for 6 hours, then pelletized and calcined at 540°C for 4 hours. The calcined sample was ion exchanged with an ammonium chloride aqueous solution with a concentration of 5% by mass at 90°C for 2 hours, washed until there was no chloride ion in the mother liquor, dried at 120°C for 6 hours, and calcined at 500°C for 4 hours to obtain catalyst D-5.
[0100] Application Examples
[0101] In a small-scale continuous flow fixed bed device, 2 g of the catalyst prepared in the above examples and comparative examples was loaded, and the catalyst performance was evaluated using pure meta-xylene (MX) reagent as the raw material. The evaluation conditions were: 270°C, 3 MPa, feed mass space velocity 3 h -1 The reaction was carried out under non-hydrogen conditions. The catalyst compositions and reaction results of the embodiments and comparative examples are shown in Tables 1 and 2.
[0102] Table 1
[0103] Catalyst No. C-1 C-2 C-3 C-4 C-5 Molecular sieve Fe / ZSM-12 Fe / ZSM-12 Fe / ZSM-12 Fe / ZSM-12 Fe / ZSM-12 <![CDATA[n(SiO2) / n(Al2O3)]]> 60 60 100 100 100 <![CDATA[n(SiO2) / n(Fe2O3)]]> 65 100 100 65 140 PX / ∑X, mass% 23.77 23.72 23.65 23.63 23.70 Xy, mass% 99.5 98.2 98.4 99.1 98.1
[0104] Table 2
[0105] Catalyst No. D-1 D-2 D-3 D-4 D-5 Molecular sieve ZSM-12 ZSM-12 ZSM-5 ZSM-11 EU-1 <![CDATA[n(SiO2) / n(Al2O3)]]> 58 88 60 60 30 PX / ∑X, mass% 23.76 23.64 23.67 23.67 23.78 Xy, mass% 98.2 98.0 98.13 97.72 96.96
[0106] Compared with the catalyst prepared in the example, the catalyst prepared in the comparative example uses a ZSM-12 molecular sieve or other molecular sieves that do not contain Fe. It can be seen from the data in Table 1 and Table 2 that the catalysts of Examples 1 to 5 prepared by the preparation method of the present invention have higher isomerization activity (PX / ∑X) for the target product p-xylene, fewer side reaction products, higher xylene yield, and better comprehensive performance than the catalysts of Comparative Examples 1 to 5, indicating that the addition of Fe in the molecular sieve synthesis by the method of the present invention can significantly improve the selectivity of the catalyst. At the same time, the pore structure of ZSM-12 is more suitable for non-hydrogen liquid phase alkyl aromatic isomerization reaction than other molecular sieves.
[0107] The present application has been described above in conjunction with the preferred embodiments, however, these embodiments are only exemplary and serve as an illustration. On this basis, various replacements and improvements can be made to the present application, all of which fall within the scope of protection of the present application.
Claims
1. A method for preparing a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst, the method comprising: (1) mixing a silicon source, an aluminum source, an iron source, a template (T) and water into a uniform mixture, and subjecting the mixture to crystallization, filtration, washing and drying to obtain a ZSM-12 molecular sieve containing Fe, wherein the silicon source is water glass, liquid silica sol or solid silica sol; (2) mixing the Fe-containing ZSM-12 molecular sieve with an inert carrier and a peptizing agent solution to form a catalyst precursor, followed by drying and calcining; and (3) exchanging the catalyst precursor with an ammonium salt, and obtaining the non-hydrogen-containing liquid phase alkyl aromatic isomerization catalyst after drying and calcining.
2. A method for preparing a non-hydrogenated liquid phase alkyl aromatic isomerization catalyst, the method comprising: (1) mixing a silicon source, an aluminum source, an iron source, a template and water into a uniform mixture, and subjecting the mixture to crystallization, filtration, washing and drying to obtain a ZSM-12 molecular sieve containing Fe, wherein the silicon source is water glass, liquid silica sol or solid silica sol; (2) exchanging the Fe-containing ZSM-12 molecular sieve with an ammonium salt, followed by drying and calcining to obtain a hydrogen-type Fe-containing ZSM-12 molecular sieve; and (3) The hydrogen-type Fe-containing ZSM-12 molecular sieve is uniformly kneaded with an inert carrier and a peptizing agent solution and formed, and then dried and calcined to obtain the non-hydrogen-containing liquid phase alkyl aromatic isomerization catalyst.
3. The method according to claim 1 or 2, wherein the molar ratio of the silicon source, aluminum source, iron source, template and water is SiO2:Al2O3:Fe2O3:T:H2O=1:(0.005~0.05):(0.005~0.05):(0.05~1):(10~60).
4. The method according to claim 1 or 2, wherein When the silicon source is water glass, the molar ratio of sodium oxide to silicon oxide in the water glass is (0.01-0.4):1; when the silicon source is liquid silica sol, the concentration of the liquid silica sol is 10-40% by mass; when the silicon source is solid silica sol, the particle size of the solid silica sol is 0.005-0.05 μm.
5. The method according to claim 4, wherein: When the silicon source is liquid silica sol, the concentration of the liquid silica sol is 20 to 40% by mass; when the silicon source is solid silica sol, the particle size of the solid silica sol is 0.01 to 0.03 μm.
6. The method according to claim 1 or 2, wherein the aluminum source is one or more selected from aluminum sulfate, aluminum chloride, aluminum acetate, and aluminum nitrate; and the iron source is one or more selected from ferric sulfate, ferric chloride, and ferric nitrate.
7. The method according to claim 1 or 2, wherein the template is a compound having the general formula N(R)4 + X - A quaternary ammonium salt, wherein R is an alkyl group with 1 to 4 carbon atoms; - is a hydroxide ion or a halogen anion; and the molar ratio of the template is X - :SiO2=0.05~1.
8. The method according to claim 7, wherein R is ethyl or propyl; X - It is a bromide ion.
9. The method according to claim 1 or 2, wherein the crystallization temperature in step (1) is 130-190°C and the crystallization time is 18-100 hours.
10. The method according to claim 9, wherein the crystallization temperature in step (1) is 140-180°C and the crystallization time is 20-96 hours.
11. The process according to claim 1 or 2, wherein the inert carrier is alumina or silica.
12. The method according to claim 1 or 2, wherein the peptizing agent is one or more selected from nitric acid, phosphoric acid, and citric acid, and the concentration of the peptizing agent solution is 1 to 5% by mass.
13. The method according to claim 1 or 2, wherein the ammonium salt is ammonium chloride or ammonium nitrate, and its use concentration is 1 to 30% by mass.
14. The method according to claim 13, wherein the ammonium salt is used at a concentration of 3 to 10% by mass.
15. The method according to any one of claims 1 to 13, wherein the drying is independently carried out at a temperature of 100 to 140°C for 4 to 24 hours; the calcination after the molding is carried out at a temperature of 520 to 550°C for 2 to 24 hours; and the calcination after the ammonium exchange is carried out at a temperature of 400 to 500°C for 2 to 24 hours.
16. A non-hydrogenated liquid phase alkyl aromatic isomerization catalyst prepared according to the method of any one of the preceding claims, the catalyst comprising: 24.0 to 99.9 mass % of a ZSM-12 molecular sieve containing Fe; and 0.1 to 76.0 mass % of an inert carrier.
17. The catalyst according to claim 16, wherein the catalyst comprises 40.0 to 70.0 mass% of the Fe-containing ZSM-12 molecular sieve.
18. The catalyst according to claim 16 or 17, wherein the Fe-containing ZSM-12 molecular sieve has a silicon-aluminum ratio of 20 to 200; and a silicon-iron ratio of 20 to 200.
19. The catalyst according to claim 18, wherein the Fe-containing ZSM-12 molecular sieve has a silicon-aluminum ratio of 30 to 150 and a silicon-iron ratio of 40 to 120.
20. The catalyst according to any one of claims 16 to 19, wherein the inert support is alumina or silica.
21. Use of the catalyst according to any one of claims 16 to 20 in the isomerization of non-hydrogenated liquid phase alkyl aromatic hydrocarbons, comprising isomerizing the alkyl aromatic hydrocarbons at 240 to 310°C and a weight hourly space velocity of 1 to 10 h at a reaction pressure that maintains the alkyl aromatic hydrocarbons in a liquid state. -1 under the conditions of , contacting with the catalyst to carry out isomerization reaction.
22. The use according to claim 21, wherein the alkyl aromatic hydrocarbon is a C8-C10 aromatic hydrocarbon.
Citation Information
Patent Citations
Xylene Isomerization Process and Catalyst Therefor
US20110263918A1
Method for preparing C8 aromatic isomerization catalyst
CN102107144A
Method for production of o-xylene from coal based raw materials
CN107266276A
Method for synthesizing ZSM-12 molecular sieves
CN108423688A
Dual-function catalyst applied to isomerization of C8 aromatic hydrocarbon and preparation method of dual-function catalyst
CN109046444A