A composite film and its preparation method and application

By adopting a multi-layer polypropylene film, combined with slip agent and impact copolymer, the problem of changes in heat sealing performance and friction coefficient of polypropylene film at high temperature is solved, and the stability and performance balance of the film at high temperature is achieved.

CN115991024BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111221981.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-11-19
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

It is difficult for existing polypropylene films to have good impact resistance, heat sealing performance and smoothness at the same time, and the heat sealing performance and friction coefficient are easily changed at high temperatures.

Method used

Using a composite film structure, including a multilayer film formed from polypropylene composition A and polypropylene composition B, which contains a slippery agent and a polyolefin elastomer, and polypropylene composition B contains random polypropylene , impact copolymer and slip agent are prepared by extrusion casting method to ensure the stability of the mechanical properties and frictional properties of the film.

Benefits of technology

The polypropylene film has achieved the stability of heat sealing performance and friction coefficient at high temperature, and has good impact resistance, heat sealing performance and smooth performance. The longitudinal tensile strength is ≥40MPa, the pendulum impact strength is ≥0.55J, 150℃ The heat sealing strength under the bottom is ≥15N/15mm, the surface friction coefficient is <0.3, and the performance changes are small after heating at 60°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003312943970000221
    Figure BDA0003312943970000221
  • Figure BDA0003312943970000231
    Figure BDA0003312943970000231
Patent Text Reader

Abstract

The present invention belongs to the field of films, and relates to a composite film and a preparation method and application thereof. The composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a, a lubricant c and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, polyolefin elastomer y, propylene impact copolymer z and a lubricant k. The composite film of the present invention has good impact resistance, heat sealing performance and lubricity, and has good heat sealing performance and friction coefficient stability after being subjected to high temperature for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of thin films, and in particular, relates to a composite thin film and a preparation method and application thereof. Background Art

[0002] Polypropylene film is often used for packaging purposes. It is required that the film has high impact resistance, good surface smoothness and low friction coefficient, which is conducive to production and winding. Polypropylene film can usually be made by methods such as casting and biaxial stretching, but polypropylene film prepared from homopolymer polypropylene raw materials usually has low impact strength. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomers can be added to polypropylene. In addition, packaging films usually need to have good heat sealing properties. The friction coefficient of the heat sealing layer material is usually high, which can easily lead to problems such as film roll adhesion.

[0003] In order to improve the impact resistance and toughness of the film, the film can be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3. The elastomer provides good impact resistance, but this method has the problem of being difficult to disperse evenly when the elastomer content is high, and the elastomer usually has poor flow properties, which may lead to uneven film performance. In order to improve the heat sealing performance of the film, a heat sealing layer is usually set in the multi-layer co-extruded film. Although the friction coefficient of the film can be reduced by adding a lubricant, a better slippery property can be obtained. However, there are still the following problems: First, it takes some time to wait for the migration and stabilization of the lubricant, and it is difficult to achieve immediate slippery performance. Moreover, if too much lubricant migrates out, it may lead to a decrease in heat sealing performance; second, if the use temperature of the film is high, the migration speed of the lubricant will become faster, resulting in a change in the slippery performance of the film.

[0004] It is difficult for existing polypropylene films to have good impact resistance, heat sealing performance and smoothness at the same time. Therefore, it is necessary to develop new polypropylene films. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good impact resistance, heat sealing performance and smoothness at the same time, and the heat sealing performance and friction coefficient change greatly due to the precipitation of the lubricant at a higher temperature, and provide a composite film and a preparation method thereof. The polypropylene film of the present invention has good impact resistance, heat sealing performance and smoothness at the same time, and after being subjected to high temperature for a long time, the heat sealing performance and friction coefficient have good stability.

[0006] The first aspect of the present invention provides a composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a, a lubricant c and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y, a propylene impact copolymer z and a lubricant k.

[0007] The second aspect of the present invention provides a method for preparing the composite film, comprising: forming the composite film by extrusion casting of a raw material composition for forming each layer after an optional granulation process.

[0008] The third aspect of the present invention provides use of the composite film in the field of packaging materials.

[0009] The composite film of the present invention has good impact resistance, heat sealing performance and smoothness, and has good heat sealing performance and friction coefficient stability after being subjected to high temperature for a long time. The longitudinal (MD) tensile strength of the film is ≥40MPa, preferably ≥52MPa; the pendulum impact strength is ≥0.55J, preferably ≥1.5J; the heat sealing strength at 150°C is ≥15N / 15mm, preferably ≥17N / 15mm; the surface friction coefficient is <0.3, preferably ≤0.23; after heating at 60°C for 24 hours, the film surface friction coefficient changes ≤0.02, preferably ≤0.01; the heat sealing strength changes ≤1N / 15mm, preferably ≤0.6N / 15mm.

[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0012] The present invention provides a composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a, a slip agent c and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y, a propylene impact copolymer z and a slip agent k.

[0013] According to some embodiments of the present invention, the composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥40MPa, preferably longitudinal tensile strength ≥52MPa; pendulum impact strength ≥0.55J, preferably pendulum impact strength ≥1.5J; heat sealing strength at 150°C ≥15N / 15mm, preferably heat sealing strength at 150°C ≥17N / 15mm; surface friction coefficient <0.3, preferably surface friction coefficient ≤0.23; after heating at 60°C for 24 hours, the surface friction coefficient of the film changes ≤0.02, preferably the surface friction coefficient of the film changes ≤0.01; heat sealing strength changes ≤1N / 15mm, preferably heat sealing strength changes ≤0.6N / 15m.

[0014] According to some embodiments of the present invention, the polypropylene a may be selected from homopolypropylene and / or propylene impact copolymer.

[0015] Preferably, the homopolypropylene has a melt mass flow rate of 2 to 15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity greater than 97%, and a molecular weight distribution Mw / Mn of 4.5 to 7.0. Homopolypropylene meeting the above characteristics is commercially available, such as homopolypropylene with a grade of PPH-FA03 from Qingdao Refining and Chemical and homopolypropylene with a grade of FC801 from Shanghai Petrochemical. Alternatively, it can be prepared by conventional methods in the art.

[0016] According to the present invention, the propylene impact copolymer is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymer part containing ethylene units, preferably selected from an ethylene-propylene copolymer part and an ethylene-butene copolymer part.

[0017] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.

[0018] Based on the total weight of the propylene impact copolymer z, the content of the copolymerized part containing ethylene units in the propylene impact copolymer z is preferably 3-15wt%. 13 C NMR determination.

[0019] The ethylene content of the propylene impact copolymer z is preferably 1-12 wt%, based on the total weight of the propylene impact copolymer z.

[0020] The propylene impact copolymer z preferably has a melt mass flow rate of 1 to 10 g / 10 min at 230° C. and a load of 2.16 kg.

[0021] The propylene impact copolymer may have a block structure or include a propylene block copolymer.

[0022] The optional propylene impact copolymer of the polypropylene a and the propylene impact copolymer z may be the same or different, preferably satisfying the above conditions.

[0023] Propylene impact copolymers meeting the above characteristics are commercially available, such as propylene impact copolymers with the brand name EP200K from Sinopec, propylene impact copolymers with the brand name M180R from Shanghai Petrochemical, and propylene impact copolymers with the brand name PPB-M02D from Maoming Petrochemical. Alternatively, they can be prepared by conventional methods in the art.

[0024] According to some embodiments of the present invention, the polyolefin elastomer b is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0025] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0026] The polyolefin elastomers meeting the above characteristics are commercially available, for example, polyolefin elastomers with the trademark of Exxon 6102, polyolefin elastomers with the trademark of Mitsui & Co., Ltd., and polyolefin elastomers with the trademark of Exxon EXACT 3139. Alternatively, they can be prepared by conventional methods in the art.

[0027] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.

[0028] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.

[0029] Random polypropylenes meeting the above characteristics are commercially available, such as Yanshan Petrochemical's F5006 random polypropylene, Shanghai Petrochemical's F500EPS random polypropylene, and Shanghai Petrochemical's F800EPS random polypropylene. Alternatively, they can be prepared by conventional methods in the art.

[0030] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 49-99.99 wt % of polypropylene a, 0-50 wt % of polyolefin elastomer b and 0.01-1 wt % of lubricant c.

[0031] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 79.8-95 wt% of polypropylene a, 4.9-20 wt% of polyolefin elastomer b and 0.08-0.2 wt% of lubricant c.

[0032] The elastomer or propylene impact copolymer in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular chain segments of the homopolymer phase of the homopolymer polypropylene or propylene impact copolymer are relatively regular, crystallization and orientation occur during the film preparation process, which provides good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the rubber phase can be evenly distributed in the film, and the size of the rubber phase in the composition can better absorb impact energy, so that the film has good impact performance; at the same time, under this ratio, the composition also contains enough homopolymer phase, so that the film has good mechanical properties.

[0033] According to some embodiments of the present invention, the lubricant c is an amide lubricant, preferably at least one of erucamide, oleamide, stearamide, behenamide, stearyl erucamide and ethylene bisstearamide.

[0034] According to some embodiments of the present invention, the lubricant k is a mixture of an amide lubricant and a migration-resistant lubricant. Wherein, the amide lubricant is preferably at least one of erucic acid amide, oleic acid amide, stearic acid amide, behenic acid amide, stearyl erucic acid amide and ethylene bis stearamide. The migration-resistant lubricant is preferably at least one of polytetrafluoroethylene particles, polyimide particles, polyamide particles, polycarbonate particles, organosilicon, nano calcium carbonate, mica and nano silicon dioxide. Preferably, the weight ratio of the amide lubricant to the migration-resistant lubricant is 1:20-1:1, preferably 1:10-1:2.

[0035] According to a preferred embodiment of the present invention, the particle size of the migration-resistant lubricant contained in the lubricant k is in the range of 0.1-5 μm, preferably 0.3-2 μm.

[0036] According to a preferred embodiment of the present invention, the molecular weight of the amide lubricant in the lubricant k is not less than the molecular weight of the amide lubricant in the lubricant d.

[0037] According to some embodiments of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B includes 39-90 wt% of random polypropylene x, 2-40 wt% of polyolefin elastomer y, 2-40 wt% of propylene impact copolymer z and 0.01-1.5 wt% of lubricant k.

[0038] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 59.4-85wt% of random polypropylene x, 4-20wt% of polyolefin elastomer y, 4-20wt% of propylene impact copolymer z and 0.08-0.6wt% of lubricant k.

[0039] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 10:1-1:4, for example, it can be 9.5:1, 9:1, 8.5:1, 8:1, 7.5:1, 7:1, 6.5:1, 6:1, 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 and any value therebetween.

[0040] According to a preferred embodiment of the present invention, the ratio of Wc to Wy is 4:1-1:4.

[0041] According to the research conducted by the present inventors, when a double-layer or multi-layer film is co-extruded, when the ratio of Wb to Wy is within the range described in the present invention, the impact resistance and optical properties of the film can be further improved, and at the same time the extrusion process will be smoother.

[0042] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min. As known to those skilled in the art, the resin component of the polypropylene composition A comprises polypropylene a and optionally a polyolefin elastomer b.

[0043] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min. As known to those skilled in the art, the resin component of the polypropylene composition B includes random polypropylene x, polyolefin elastomer y and propylene impact copolymer z.

[0044] When the melt mass flow rates of the resin components of the polypropylene composition A and the resin components of the polypropylene composition B are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity, mechanical properties and optical properties.

[0045] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A, the resin component of the film A, the film layer B or the resin component of the film layer B, or may have different compositions from the film layer A, the resin component of the film A, the film layer B or the resin component of the film layer B, or may be a mixture of the polypropylene composition A and the polypropylene composition B or their resin components. When the composite film has a structure of three or more layers, the film layer B is preferably used as a surface layer, such as a three-layer film including the film layer A, the film layer B, and the film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.

[0046] According to some embodiments of the present invention, in the composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.

[0047] According to a preferred embodiment of the present invention, in the composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:3-1:1. Under this ratio, the composite film has good mechanical properties.

[0048] Polyolefin elastomers can improve the impact performance of the film, but when added in large amounts, they will separate from the matrix, resulting in an increase in the film's surface friction coefficient. Usually, the film's surface friction coefficient can be reduced and the film's slip performance can be improved by adding a lubricant to the surface or inside of the film. However, usually, because the lubricant takes time to migrate to the film surface, the film needs to be placed for a certain period of time to achieve qualified slip performance. Moreover, if the film needs to be placed or matured in a high temperature environment (above 40°C), the high temperature will further accelerate the migration of the lubricant, resulting in the lubricant migrating out too quickly in the early stage of placement, and the friction coefficient is reduced too much, which may affect the heat sealing or corona performance. After the lubricant is consumed in the later stage, the film's friction coefficient begins to increase again, and the friction coefficient changes greatly over time.

[0049] On the one hand, the present invention improves the initial slip performance of the film by adding a composite slip agent to the surface layer containing the polypropylene composition B. The migration-resistant slip agent part in the composite slip agent can provide a part of the slip performance without the need for a precipitation process. By adjusting the particle size range, it is ensured that the heat sealing performance and optical properties of the film will not change. In addition, the amide slip agent in the surface layer can also provide a certain slip performance, further reduce the friction coefficient of the film, and improve the initial slip performance of the film.

[0050] On the other hand, the present invention provides good high-temperature slip and heat-sealing performance retention through the use of a composite lubricant and the combination of a core surface layer lubricant. The composite lubricant used in the film surface layer of the present invention can not only improve the initial slip performance, but also delay the precipitation of the core layer lubricant when the migration-resistant lubricant is evenly distributed on the film surface. Further, by regulating the type and content of the amide lubricant of the surface layer and the core layer, the molecular weight of the surface layer amide lubricant is not less than the molecular weight of the core layer amide lubricant, which can not only slow down the precipitation speed of the surface layer lubricant, but also further adjust the precipitation balance of the lubricant through the surface layer lubricant. Finally, a good high-temperature slip and heat-sealing performance retention effect is achieved.

[0051] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.

[0052] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A and the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.

[0053] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A and the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.

[0054] According to the present invention, in order to improve other properties of the composite film (such as stability, antistatic property, etc.), the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, an antistatic agent, and an anti-adhesive agent (anti-adhesive agent). The specific type of the film-forming aid can be a conventional choice in the art, and the present invention is not particularly limited thereto.

[0055] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.

[0056] The present invention also provides a method for preparing the composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0057] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.

[0058] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.

[0059] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.

[0060] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.

[0061] The composite film of the present invention can be used in the field of packaging materials, such as high-end packaging fields that have high requirements on film impact resistance, optical properties and performance, including but not limited to battery packaging, electronic product packaging or high-end food packaging.

[0062] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.

[0063] In the following examples and comparative examples:

[0064] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.

[0065] The properties of the polypropylene composition and film were tested according to the following method: the film was tested after being placed at 23° C. for 48 hours, and the test results are shown in Table 1; the film was tested after being placed in an oven at 60° C. for 24 hours, and the test results are shown in Table 2.

[0066] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.

[0067] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.

[0068] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.

[0069] (4) Film haze: measured according to the method specified in GB / T 2410-2008.

[0070] (5) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.

[0071] (6) Film friction coefficient: measured according to the method specified in GB / T1006-1988.

[0072] (7) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.

[0073] (8) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.

[0074] Example 1

[0075] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0076] (1) Preparation of polypropylene composition A:

[0077] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is a polyolefin elastomer with the brand name 6102, purchased from Exxon, an ethylene-propylene copolymer, and an ethylene structural unit content of 16wt%; and lubricant c is erucic acid amide, purchased from Aladdin Reagent Company. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then, lubricant c and lubricant (the lubricant is a PEG lubricant produced by Clariant, Switzerland, with a molecular weight of 10000) are added, and the amount of lubricant c added is 0.1 parts by weight, and the amount of lubricant added is 0.1 parts by weight, based on the sum of the mass of the above-mentioned components a and b as 100 parts by weight. Then, the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. The screw is melt-mixed, extruded, granulated and dried to obtain a polypropylene composition A pellet. The melt mass flow rate MFR of the resin component is tested. A =3.5g / 10min.

[0078] (2) Preparation of polypropylene composition B:

[0079] Component x is a random polypropylene with a brand name of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer with a brand name of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16 wt%; component z is a propylene impact copolymer with a brand name of EP200K, purchased from China Sands Petrochemical, with an ethylene content of 8 wt%, an ethylene-propylene copolymer content of 13 wt%, and a melt mass flow rate of 3.2 g / 10 min; and lubricant k is stearyl erucic acid amide and polytetrafluoroethylene particles (the mass ratio of stearyl erucic acid amide to polytetrafluoroethylene particles is 1:5, stearyl erucic acid amide is purchased from Jiangxi Dongyuan Company, and polytetrafluoroethylene particles are purchased from Solvay Group with a particle size of 1-2 μm). The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. The sum of the masses of the above components x, y and z is 100 parts by weight, and the amount of lubricant k added is 0.4 parts by weight. Wb:Wy is 4:1. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR of its resin component is tested. B =4.7g / 10min.

[0080] (3) Preparation of composite films:

[0081] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition B is introduced into the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition A is added into the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added into the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer A) and a core layer (film layer B). The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 2:1.

[0082] Example 2

[0083] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0084] (1) Preparation of polypropylene composition A:

[0085] Component a is a propylene impact copolymer with the brand name M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; component b is a polyolefin elastomer with the brand name DF640, purchased from Mitsui Company, and is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%; lubricant c is oleic acid amide, purchased from Jiangsu Zhongteng New Materials Co., Ltd. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Then add lubricant c and lubricant (the lubricant is a PEG lubricant produced by Clariant, Switzerland, with a molecular weight of 10000), based on the sum of the mass of the above-mentioned components a and b as 100 parts by weight, the amount of lubricant c added is 0.2 parts by weight, and the amount of lubricant added is 0.1 parts by weight. Then, the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. The screw is melt-mixed, extruded, granulated and dried to obtain a polypropylene composition A pellet. The melt mass flow rate MFR of the resin component is tested. A =3.1g / 10min.

[0086] (2) Preparation of polypropylene composition B:

[0087] Component x is a random polypropylene with a brand name of F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3g / 10min; component y is a polyolefin elastomer with a brand name of DF640, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%; component z is a propylene impact copolymer with a brand name of M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; lubricant k is stearyl erucic acid amide and polytetrafluoroethylene particles (the mass ratio of ethylene bisstearamide and polytetrafluoroethylene particles is 1:10, ethylene bisstearamide is purchased from Jiangsu Zhongteng New Materials, and polytetrafluoroethylene particles are purchased from Solvay Group with a particle size of 1-2μm). The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. The sum of the masses of the above components x, y and z is 100 parts by weight, and the amount of lubricant k added is 0.1 parts by weight. Wb:Wy is 1:4. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR of its resin component is tested.B =4.5g / 10min.

[0088] (3) Preparation of composite films:

[0089] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition A is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer A) and a core layer (film layer B). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.

[0090] Example 3

[0091] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0092] (1) Preparation of polypropylene composition A:

[0093] Component a is a homopolymer polypropylene with a grade of FC801, purchased from Shanghai Petrochemical, with a melt mass flow rate of 7.8g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.8; component b is a polyolefin elastomer with a grade of EXACT3139, purchased from Exxon, and is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%; lubricant c is stearic acid amide, purchased from Jiangsu Zhongteng New Materials Co., Ltd. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 85 parts by weight, and the mass fraction Wb of component b is 15 parts by weight. Then add lubricant c and lubricant (the lubricant is a PEG lubricant produced by Clariant, Switzerland, with a molecular weight of 10000), based on the sum of the mass of the above-mentioned components a and b as 100 parts by weight, the amount of lubricant c added is 0.15 parts by weight, and the amount of lubricant added is 0.1 parts by weight. Then, the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. The screw is melt-mixed, extruded, granulated and dried to obtain a polypropylene composition A pellet. The melt mass flow rate MFR of the resin component is tested. A =7.9g / 10min.

[0094] (2) Preparation of polypropylene composition B:

[0095] Component x is a random polypropylene with a brand name of F800EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 8.2 g / 10 min; component y is a polyolefin elastomer with a brand name of EXACT3139, purchased from Exxon, which is an ethylene-1-octene copolymer with an octene structural unit content of 14 wt%; component z is a propylene impact copolymer with a brand name of PPB-M02D, purchased from Maoming Petrochemical, with an ethylene content of 8 wt%, an ethylene-propylene copolymer content of 10 wt%, and a melt mass flow rate of 1.5 g / 10 min; and lubricant k is behenic acid amide and silica particles (the mass ratio of behenic acid amide to silica particles is 1:2, behenic acid amide is purchased from West Asia Reagent Company, and silica particles are purchased from Quanzhou Haida New Materials Company, with a particle size of 0.3-1 μm). The components prepared above were weighed and mixed according to the proportions, wherein the mass fraction Wx of component x was 85 parts by weight, the mass fraction Wy of component y was 10 parts by weight, the mass fraction Wz of component z was 5 parts by weight, and the amount of lubricant k added was 0.6 parts by weight. Wb:Wy was 3:2. The other steps were the same as step (1), and finally a polypropylene composition B pellet was obtained. The melt mass flow rate MFR of its resin component was tested. B =7.4g / 10min.

[0096] (3) Preparation of composite films:

[0097] The preparation process is the same as step (3) of Example 1.

[0098] Example 4

[0099] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0100] (1) Preparation of polypropylene composition A:

[0101] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. The amount of lubricant c added is 0.05 parts by weight. The pellets of polypropylene composition A are obtained, and the melt mass flow rate MFR of the resin component is tested. A =3.2g / 10min.

[0102] (2) Preparation of polypropylene composition B:

[0103] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, the mass fraction Wz of component z is 5 parts by weight, and the amount of lubricant k added is 0.8 parts by weight. Wb:Wy is 6:1. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR of its resin component is tested. B =8.3g / 10min.

[0104] (3) Preparation of composite films:

[0105] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.

[0106] Example 5

[0107] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0108] (1) Preparation of polypropylene composition A:

[0109] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. The amount of lubricant c added is 0.05 parts by weight. The pellets of polypropylene composition A are obtained, and the melt mass flow rate MFR of the resin component is tested. A =9.3g / 10min.

[0110] (2) Preparation of polypropylene composition B:

[0111] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 12 parts by weight, the mass fraction Wz of component z is 3 parts by weight, and the amount of lubricant k added is 1 part by weight. Wb:Wy is 25:12. Finally, the polypropylene composition B pellets are obtained, and the melt mass flow rate MFR of the resin component is tested. B =9.2g / 10min.

[0112] (3) Preparation of composite films:

[0113] The steps are the same as those in Example 2. The film thickness is 50 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 2:1.

[0114] Example 6

[0115] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0116] (1) Preparation of polypropylene composition A:

[0117] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 100 parts by weight. The amount of lubricant c added is 0.3 parts by weight. The pellets of polypropylene composition A are obtained, and the melt mass flow rate MFR of the resin component is tested. A =7.8g / 10min.

[0118] (2) Preparation of polypropylene composition B:

[0119] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 30 parts by weight, the mass fraction Wz of component z is 20 parts by weight, and the amount of lubricant k added is 0.05 parts by weight. Finally, pellets of polypropylene composition B are obtained. The melt mass flow rate MFR of the resin component is tested. B =6.8g / 10min.

[0120] (3) Preparation of composite films:

[0121] The steps are the same as those in Example 3. The film thickness is 50 μm, wherein the ratio of the thickness of the upper surface layer to the thickness of the core layer is 1:4.

[0122] Example 7

[0123] This example is used to illustrate the preparation of the composite film provided by the present invention.

[0124] (1) Preparation of polypropylene composition A:

[0125] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 100 parts by weight. The pellets of polypropylene composition A are obtained. The melt mass flow rate MFR of the resin component is tested. A =3.1g / 10min.

[0126] (2) Preparation of polypropylene composition B:

[0127] The steps are the same as those in Example 1, except that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 30 parts by weight, the mass fraction Wz of component z is 20 parts by weight, and the amount of lubricant k added is 0.05 parts by weight. Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate MFR thereof is tested. B =3.5g / 10min.

[0128] (3) Preparation of composite films:

[0129] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.

[0130] Example 8

[0131] The composite film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition A, the mass fraction Wa of component a was 100 parts by weight. Finally, the polypropylene composition A pellets were obtained. The melt mass flow rate MFR of the resin component was tested. A =3.1g / 10min.

[0132] Example 9

[0133] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 50 parts by weight, and the mass fraction Wb of component b is 50 parts by weight. Wb:Wy is 10:1. Finally, pellets of polypropylene composition A were obtained. The melt mass flow rate MFR of its resin component was tested. A =3.5g / 10min.

[0134] Example 10

[0135] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 40 parts by weight, the mass fraction Wy of component y is 30 parts by weight, the mass fraction Wz of component z is 30 parts by weight, and the amount of lubricant k added is 1 part by weight. Wb:Wy is 2:3. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin component was tested. B =4.5g / 10min.

[0136] Embodiment 11

[0137] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 40 parts by weight, the mass fraction Wz of component z is 10 parts by weight, and the amount of lubricant k added is 1 part by weight. Wb:Wy is 1:2. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin component was tested. B =5.0g / 10min.

[0138] Example 12

[0139] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wz of component z is 40 parts by weight. Wb:Wy is 2:1. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin components thereof was tested. B =4.8g / 10min.

[0140] Example 13

[0141] The composite film was prepared according to the method of Example 1. The difference was that in the preparation of polypropylene composition A, the mass fraction Wa of component a was 99 parts by weight, and the mass fraction Wb of component b was 1 part by weight. The ratio of Wb:Wy was 1:5. Finally, the pellets of polypropylene composition B were obtained. The melt mass flow rate MFR of the resin component was tested. A =3.2g / 10min.

[0142] Embodiment 14

[0143] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 97.5 parts by weight, and the mass fraction Wb of component b is 2.5 parts by weight. Wb:Wy is 1:2. Finally, polypropylene composition B pellets were obtained. The melt mass flow rate MFR of the resin component was tested. A =3.1g / 10min.

[0144] Embodiment 15

[0145] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Wb:Wy is 1:1. Finally, pellets of polypropylene composition B were obtained. The melt mass flow rate MFR of its resin component was tested. A =3.2g / 10min.

[0146] Example 16

[0147] The composite film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition A, the mass fraction Wa of component a was 90 parts by weight, and the mass fraction Wb of component b was 10 parts by weight. Wb:Wy was 2:1. Finally, the pellets of the polypropylene composition B were obtained. The melt mass flow rate MFR of the resin component was tested. A =3.3g / 10min.

[0148] Embodiment 17

[0149] A composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. Wb:Wy is 5:1. Finally, pellets of polypropylene composition B were obtained. The melt mass flow rate MFR of its resin component was tested. A =3.1g / 10min.

[0150] Comparative Example 1

[0151] A composite film was prepared according to the method of Example 1. The difference was that only the polypropylene composition A was used for extrusion casting into a single-layer film, and the film thickness was 50 μm.

[0152] Comparative Example 2

[0153] A composite film was prepared according to the method of Example 2, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 50 μm.

[0154] Comparative Example 3

[0155] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x.

[0156] Comparative Example 4

[0157] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x and component y, wherein the mass fraction Wx of component x was 85 parts by weight, and the mass fraction Wy of component y was 15 parts by weight.

[0158] Comparative Example 5

[0159] A composite film was prepared according to the method of Example 2. The difference was that the polypropylene composition B contained only component x and component z, wherein the mass fraction Wx of component x was 70 parts by weight, and the mass fraction Wz of component z was 30 parts by weight.

[0160] Comparative Example 6

[0161] A composite film was prepared according to the method of Example 2. The difference was that the polypropylene composition B contained only component x and component k, wherein the mass fraction Wx of component x was 98 parts by weight, and the mass fraction Wk of component k was 2 parts by weight.

[0162] Comparative Example 7

[0163] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition A did not contain the lubricant c, and the polypropylene composition B did not contain the lubricant k.

[0164] Comparative Example 8

[0165] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition A did not contain the lubricant c.

[0166] Comparative Example 9

[0167] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B did not contain the lubricant k.

[0168] Table 1

[0169]

[0170] Table 2

[0171]

[0172] It can be seen from the results in Table 1 that the composite film provided by the present invention has excellent impact resistance, optical properties and tensile properties at the same time, and has excellent heat sealing strength. The longitudinal (MD) tensile strength of the film of the present invention is ≥40MPa, the surface friction coefficient is <0.3, the pendulum impact strength is ≥0.55J, and the heat sealing strength at 150°C is ≥15N / 15mm. It can be seen from the preferred embodiments that the longitudinal (MD) tensile strength of the film of the present invention is ≥52MPa, preferably ≤0.23, the pendulum impact strength is ≥1.5J, and the heat sealing strength at 150°C is ≥17N / 15mm. It can be seen from the comparative examples that it is difficult to achieve a balance of various properties by only using a single-layer film or changing the ratio of the film layer components, and during extrusion casting, the film surface is unstable, and it is difficult to obtain a film with uniform thickness.

[0173] It can be seen from the results in Table 2 that after heating at 60° C. for 24 hours, the film surface friction coefficient changes by ≤0.02, preferably ≤0.01; and the heat seal strength changes by ≤1 N / 15 mm, preferably ≤0.6 N / 15 mm.

[0174] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0175] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A composite film, characterized in that: The composite film is composed of at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a, a slip agent c and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y, a propylene impact copolymer z and a slip agent k; Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 49-99.99wt% of polypropylene a, 0-50wt% of polyolefin elastomer b and 0.01-1wt% of lubricant c; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 39-90wt% of random polypropylene x, 2-40wt% of polyolefin elastomer y, 2-40wt% of propylene impact copolymer z and 0.01-1.5wt% of lubricant k; When the polypropylene composition A includes the polyolefin elastomer b, based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 10:1-1:4; The polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an alpha olefin; the propylene impact copolymer z is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer z, the ethylene content of the propylene impact copolymer z is 1-12wt%.

2. The composite film according to claim 1, characterized in that The composite film has at least one of the following characteristics: longitudinal tensile strength ≥40MPa; pendulum impact strength ≥0.55J; heat sealing strength at 150°C ≥15N / 15mm; surface friction coefficient <0.3; after heating at 60°C for 24 hours, the film surface friction coefficient changes ≤0.02; heat sealing strength changes ≤1N / 15mm.

3. The composite film according to claim 2, characterized in that: The longitudinal tensile strength is ≥52MPa.

4. The composite film according to claim 2, characterized in that: The pendulum impact strength is ≥1.5J.

5. The composite film according to claim 2, characterized in that: The heat sealing strength at 150° C. is ≥17N / 15mm.

6. The composite film according to claim 2, characterized in that: The surface friction coefficient is ≤0.

23.

7. The composite film according to claim 2, characterized in that: The film surface friction coefficient changes by ≤0.

01.

8. The composite film according to claim 2, characterized in that: The heat seal strength variation is ≤0.6N / 15mm.

9. The composite film according to claim 1, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min.

10. The composite film according to claim 9, characterized in that At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 3-8 g / 10 min.

11. The composite film according to claim 9, characterized in that At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 4-8 g / 10 min.

12. The composite film according to claim 1, characterized in that: The polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.

13. The composite film according to claim 12, characterized in that: The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.

0.

14. The composite film according to claim 12, characterized in that: The propylene impact copolymer is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer, the ethylene content of the propylene impact copolymer is 1-12wt%; The copolymerization part containing ethylene units in the propylene impact copolymer has a content of 3-15wt%; The propylene impact copolymer has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

15. The composite film according to claim 1, characterized in that The alpha olefin is C3-C 12 of alpha olefins.

16. The composite film according to claim 15, characterized in that The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

17. The composite film according to claim 1, characterized in that The lubricant c is an amide lubricant.

18. The composite film according to claim 17, characterized in that The lubricant c is at least one of erucamide, oleamide, stearamide, behenamide, stearyl erucamide and ethylene bisstearamide.

19. The composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.

20. The composite film according to claim 19, characterized in that The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.

21. The composite film according to claim 1, characterized in that The copolymerization part containing ethylene units in the propylene impact copolymer z has a content of 3-15wt%; The propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

22. The composite film according to claim 1, characterized in that The lubricant K is a mixture of an amide lubricant and a migration-resistant lubricant.

23. The composite film according to claim 22, characterized in that The amide lubricant is at least one of erucamide, oleamide, stearamide, behenamide, stearyl erucamide and ethylene bisstearamide.

24. The composite film according to claim 22, characterized in that The migration-resistant lubricant is at least one of polytetrafluoroethylene particles, polyimide particles, polyamide particles, polycarbonate particles, organic silicon, nano calcium carbonate, mica and nano silicon dioxide.

25. The composite film according to claim 22, characterized in that The weight ratio of the amide lubricant to the migration-resistant lubricant is 1:20 to 1:

1.

26. The composite film according to claim 25, characterized in that The weight ratio of the amide lubricant to the migration-resistant lubricant is 1:10 to 1:

2.

27. The composite film according to claim 22, characterized in that The particle size of the migration-resistant lubricant ranges from 0.1 to 5 μm.

28. The composite film according to claim 27, characterized in that The particle size of the migration-resistant lubricant is in the range of 0.3 to 2 μm.

29. The composite film according to claim 1, characterized in that The molecular weight of the amide lubricant in the lubricant k is not less than the molecular weight of the amide lubricant in the lubricant c.

30. The composite film according to claim 1, characterized in that Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 79.8-95 wt% of polypropylene a, 4.9-20 wt% of polyolefin elastomer b and 0.08-0.2 wt% of lubricant c.

31. The composite film according to claim 1, characterized in that Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 59.4-85 wt% of random polypropylene x, 4-20 wt% of polyolefin elastomer y, 4-20 wt% of propylene impact copolymer z and 0.08-0.6 wt% of lubricant k.

32. The composite film according to claim 1, characterized in that Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 4:1-1:

4.

33. The composite film according to any one of claims 1 to 32, characterized in that: In the composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:

1.

34. The composite film according to claim 33, characterized in that In the composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:3-1:

1.

35. The composite film according to any one of claims 1 to 32, characterized in that: When the composite film has a structure of three or more layers, the film layer B is the surface layer.

36. The composite film according to any one of claims 1 to 32, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.

37. The composite film according to claim 36, characterized in that The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.

38. The composite film according to claim 36, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.

39. The composite film according to claim 38, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.

40. The composite film according to claim 36, characterized in that The lubricant is a PEG lubricant and / or a monoglyceride lubricant.

41. The composite film according to claim 36, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.

42. The composite film according to claim 41, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.

43. The composite film according to any one of claims 1 to 32, characterized in that The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.

44. The composite film according to claim 43, characterized in that The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, an antistatic agent and an anti-sticking agent.

45. The composite film according to claim 43, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.

46. ​​The composite film according to claim 45, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.

47. A method for preparing a composite film according to any one of claims 1 to 46, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.

48. The preparation method according to claim 47, characterized in that The stretching is bidirectional stretching.

49. Use of the composite film according to any one of claims 1 to 46 in the field of packaging materials.