Antistatic polypropylene composite film and preparation method and application thereof
By adopting a double-layer or multi-layer structure in polypropylene film, combining polyolefin elastomer and conductive filler, the problem of insufficient impact resistance, stretching, heat sealing and electrostatic properties in packaging purposes is solved, and a high degree of Performance antistatic polypropylene composite film suitable for high-end packaging fields.
Patent Information
- Application Number
- CN202111223354.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-20
AI Technical Summary
Polypropylene films have problems in insufficient impact resistance, tensile properties, heat sealing properties and anti-static properties in packaging applications, especially at high heat sealing temperatures, low heat sealing strength and prone to electrostatic accumulation, leading to problems in production and application.
Anti-static polypropylene composite film with a double-layer or multi-layer structure, combining homopolypolypropylene and propylene impact copolymerization by adding polyolefin elastomer to polypropylene composition A and adding conductive filler to polypropylene composition B. to form a thin film with good mechanical properties and electrical conductivity.
The film has achieved high heat seal strength, good impact resistance and anti-static properties at lower heat sealing temperatures, with longitudinal tensile strength ≥45MPa, pendulum impact strength ≥0.6J, and surface resistivity is 102-108Ω, suitable for high-end Packaging field.
Smart Images

Figure BDA0003313418720000151 
Figure BDA0003313418720000161
Abstract
Description
Technical Field
[0001] The invention belongs to the field of films, and in particular relates to an antistatic polypropylene composite film and a preparation method and application thereof. Background Art
[0002] Polypropylene film can usually be made by casting and biaxial stretching, but the impact strength of polypropylene film made from homopolymer polypropylene raw materials is usually low. Polypropylene film is often used for packaging purposes, which requires the film to have high impact performance. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomer can be added to polypropylene, but the films prepared by the above methods usually have high haze. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.
[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3. The elastomer provides good impact resistance. However, this method has the problem of difficulty in uniform dispersion when the elastomer content is high, and the amount of elastomer added will be limited, because when the amount added reaches a certain level, phase separation will occur, thereby limiting the further improvement of impact performance. Moreover, when the film is used for packaging purposes, it is usually hoped that it has good heat sealing performance at a lower heat sealing temperature.
[0004] Polypropylene molecules are completely non-polar and highly electrically insulating. Their surface resistivity is 10 16 -10 17 Ω, volume resistivity is 10 16 -10 18Ω / cm, it is easy to generate static charge accumulation, which will cause the polypropylene film to carry static electricity due to friction and other reasons during the production or processing of the film, which is difficult to eliminate through conduction, causing problems for the production, processing, storage, transportation and application of the film. For example, when using film to package powdered goods, the sealing strength is often greatly reduced due to static dust absorption on the heat-sealed surface, and the goods will be seriously damaged during storage and transportation; when the film is printed, the electrostatic dust absorption effect of the film may affect the ink transfer, resulting in uneven ink "static ink spots" and other defects in the printed pattern; during the packaging process of the high-speed packaging production line, static electricity will affect the cutting, transportation, folding, etc. of the film; especially with the rapid development of the IT industry, various sensitive electronic components, instruments and meters are also widely packaged with plastic film. The film will accumulate static electricity due to electromagnetic induction and friction, causing the packaged goods to be damaged by the high-voltage discharge generated by it. Antistatic polypropylene film was first used in powder packaging, food packaging, candy packaging and other fields. After the 1980s, antistatic polypropylene film and products developed rapidly in the fields of electromechanical products, instrument components, electronic components, large-scale integrated circuits, circuit boards, etc., and the demand and usage increased rapidly.
[0005] Therefore, there is a need in the art to develop a polypropylene film that has good impact resistance, tensile strength, heat sealing performance and antistatic properties. Summary of the invention
[0006] The purpose of the present invention is to provide a high impact heat-seal antistatic polypropylene composite film and a preparation method thereof. The antistatic polypropylene composite film of the present invention has good impact resistance, tensile properties, antistatic properties, and good heat-seal strength at a relatively low heat-seal temperature.
[0007] The first aspect of the present invention provides an antistatic polypropylene composite film, which includes at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A includes polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B includes a resin component and a conductive filler, and the resin component includes a random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z.
[0008] The second aspect of the present invention provides a method for preparing the antistatic polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0009] The third aspect of the present invention provides application of the antistatic polypropylene composite film in the field of packaging materials.
[0010] The antistatic composite film of the present invention has good impact resistance, tensile properties and antistatic properties, and has good heat sealing strength at a relatively low heat sealing temperature. The longitudinal (MD) tensile strength of the film is ≥45MPa, preferably ≥52MPa; the pendulum impact strength is ≥0.6J, preferably ≥1.5J; the heat sealing strength at 150°C is ≥15N / 15mm, preferably ≥18N / 15mm; the surface resistivity is 10 2 -10 8 Ω, the preferred surface resistivity is 10 2 -10 4 Ω.
[0011] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0012] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0013] The present invention provides an antistatic polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, the polypropylene composition B comprises a resin component and a conductive filler, and the resin component comprises a random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z.
[0014] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥45MPa, preferably longitudinal (MD) tensile strength ≥52MPa; pendulum impact strength ≥0.6J, preferably pendulum impact strength ≥1.5J; heat sealing strength at 150°C ≥15N / 15mm, preferably heat sealing strength at 150°C ≥18N / 15mm; surface resistivity ≥10 2 -10 8 Ω, the preferred surface resistivity is 10 2 -10 4 Ω.
[0015] According to some embodiments of the present invention, the polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.
[0016] Preferably, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available, such as the homopolypropylene with the grade PPH-FA03 of Qingdao Refining and Chemical Co., Ltd. Alternatively, it can be prepared by conventional methods in the art.
[0017] According to the present invention, the propylene impact copolymer is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymer part containing ethylene units, preferably selected from an ethylene-propylene copolymer part and an ethylene-butene copolymer part.
[0018] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.
[0019] Based on the total weight of the propylene impact copolymer z, the content of the copolymerized part containing ethylene units in the propylene impact copolymer z is preferably 3-15wt%. 13 C NMR determination.
[0020] The ethylene content of the propylene impact copolymer z is preferably 1-12 wt%, based on the total weight of the propylene impact copolymer z.
[0021] The propylene impact copolymer z preferably has a melt mass flow rate of 1 to 10 g / 10 min at 230° C. and a load of 2.16 kg.
[0022] The propylene impact copolymer may have a block structure or include a propylene block copolymer.
[0023] The optional propylene impact copolymer of the polypropylene a and the propylene impact copolymer z may be the same or different, preferably satisfying the above conditions.
[0024] The propylene impact copolymers meeting the above characteristics are commercially available, such as the propylene impact copolymers with the brand name EP200K of Sinopec and the propylene impact copolymers with the brand name M180R of Shanghai Petrochemical, or can be prepared by conventional methods in the art.
[0025] According to some embodiments of the present invention, the polyolefin elastomer b is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
[0026] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
[0027] The polyolefin elastomer meeting the above characteristics is commercially available, for example, the polyolefin elastomer with the brand number 6102 from Exxon and the polyolefin elastomer with the brand number DF640 from Mitsui, or can be prepared by conventional methods in the art.
[0028] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.
[0029] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.
[0030] Random polypropylene meeting the above characteristics is commercially available, such as Yanshan Petrochemical's F5006 random polypropylene and Shanghai Petrochemical's F500EPS random polypropylene, or can be prepared by conventional methods in the art.
[0031] According to some embodiments of the present invention, the conductive filler may be a conventional choice in the art, for example, it may be at least one of carbon black conductive fillers, graphite conductive fillers, carbon nanotube conductive fillers, carbon fiber conductive fillers, conductive metal particles, conductive metal fibers and metal oxides. Wherein, the carbon black conductive filler includes but is not limited to at least one of acetylene black, superconducting carbon black and special conductive carbon black. The graphite conductive filler includes but is not limited to at least one of natural graphite, expandable graphite, expanded graphite and graphene. The carbon nanotube conductive filler includes but is not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes that are not surface-modified or surface-modified. Wherein, the surface modification method is well known to those skilled in the art and is not described here. The conductive metal in the conductive metal particles and conductive metal fibers may be independently at least one of silver, aluminum, copper, iron, nickel and stainless steel. The filler coated with conductive metal may be selected from at least one of lead-plated, nickel-plated, silver-plated glass balls, glass fibers and mica sheets. The metal oxide includes but is not limited to at least one of titanium oxide, zinc oxide, tin oxide, indium oxide and cadmium oxide. The polypropylene antistatic film is prepared by adding conductive fillers, and its antistatic property is long-lasting and is less affected by environmental humidity.
[0032] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 70-100 wt % of the polypropylene a and 0-30 wt % of the polyolefin elastomer b.
[0033] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 80-95 wt% of polypropylene a and 5-20 wt% of polyolefin elastomer b.
[0034] The elastomer or propylene impact copolymer in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular segments of the homopolymerized phase part of the homopolymerized polypropylene and the propylene impact copolymer are relatively regular, crystallization and orientation occur during the film preparation process, providing good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the size of the rubber phase in the composition can absorb impact energy well, meet the requirements of impact performance, and make the film have good impact performance. At the same time, since the macromolecular segments of the homopolymerized phase part are relatively regular, crystallization occurs during the film preparation process, so the film also has good tensile properties.
[0035] According to some embodiments of the present invention, in the polypropylene composition B, the content of the conductive filler is 0.1-10 parts by weight, based on 100 parts by weight of the resin component, and the resin component includes 50-90wt% of random polypropylene x, 5-35wt% of polyolefin elastomer y, and 2-30wt% of propylene impact copolymer z.
[0036] According to a preferred embodiment of the present invention, based on 100 parts by weight of the resin component, the content of the conductive filler is 0.5-4.5 parts by weight, and the resin component includes 60-85wt% of random polypropylene x, 5-20wt% of polyolefin elastomer y, and 5-20wt% of propylene impact copolymer z.
[0037] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:6, for example, it can be 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 and any value therebetween.
[0038] According to a preferred embodiment of the present invention, the ratio of Wb to Wy is 4:1-1:4.
[0039] According to the research conducted by the present inventors, when a double-layer or multi-layer film is co-extruded, when the ratio of Wb to Wy is within the range of the present invention, the impact performance of the film can be further improved, and at the same time the extrusion process will be more stable.
[0040] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min.
[0041] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min.
[0042] When the melt mass flow rate of the resin components of the polypropylene composition A and the polypropylene composition B is within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity and mechanical properties.
[0043] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A, the film layer B, or the resin component of the film layer B, or may have a different composition from the resin component of the film layer A, the film layer B, or the film layer B, or may be a mixture of the resin components of the polypropylene composition A and the polypropylene composition B. When the polypropylene composite film has a structure of more than three layers, the film layer B is preferably used as the surface layer, such as a three-layer film including the film layer A, the film layer B, and the film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.
[0044] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.
[0045] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:3-1:1. Under this ratio, the composite film has good mechanical properties.
[0046] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.
[0047] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.
[0048] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.
[0049] According to the present invention, in order to improve other properties (such as stability, etc.) of the composite film, the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, and an anti-adhesive agent (anti-adhesive agent). The specific type of the film-forming aid can be a conventional choice in the art, and the present invention is not particularly limited thereto.
[0050] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.
[0051] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0052] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.
[0053] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.
[0054] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.
[0055] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.
[0056] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as high-end packaging fields that require high impact resistance and antistatic properties of the film, including but not limited to battery packaging, electronic product packaging, industrial powder packaging or high-end food packaging.
[0057] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0058] In the following examples and comparative examples:
[0059] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.
[0060] The polypropylene composition and antistatic film properties were tested according to the following method, and the film test results are shown in Table 1:
[0061] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.
[0062] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.
[0063] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.
[0064] (4) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.
[0065] (5) Film surface resistivity: tested by Keithley 6517B Electrometer.
[0066] (6) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland.13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.
[0067] (7) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.
[0068] Example 1
[0069] This example is used to illustrate the preparation of the antistatic composite film provided by the present invention.
[0070] (1) Preparation of polypropylene composition A:
[0071] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is polyolefin elastomer with the brand name 6102, purchased from Exxon, and is an ethylene-propylene copolymer with an ethylene structural unit content of 16 wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.5g / 10min.
[0072] (2) Preparation of polypropylene composition B:
[0073] Component x is a random polypropylene with a grade of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2g / 10min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%; component z is a propylene impact copolymer with a grade of EP200K, purchased from China Sands Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 13wt%, and a melt mass flow rate of 3.2g / 10min; the conductive filler is a multi-walled carbon nanotube purchased from Cheap Tubes, USA. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. Wb:Wy is 4:1. Based on 100 parts by weight of the resin, the carbon nanotubes are 3 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR of the resin component is tested. B =4.7g / 10min.
[0074] (3) Preparation of composite films:
[0075] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.
[0076] Example 2
[0077] This example is used to illustrate the preparation of the antistatic composite film provided by the present invention.
[0078] (1) Preparation of polypropylene composition A:
[0079] Component a is a propylene impact copolymer with the brand name M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; component b is a polyolefin elastomer with the brand name DF640, purchased from Mitsui Co., Ltd., an ethylene-1-butene copolymer, with a butene structural unit content of 32wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.1g / 10min.
[0080] (2) Preparation of polypropylene composition B:
[0081] Component x is a random polypropylene with the brand name F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3g / 10min; component y is a polyolefin elastomer with the brand name DF640, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%; component z is a propylene impact copolymer with the brand name M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; the conductive filler is graphene, which is self-made. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. Wb:Wy is 1:4. Based on 100 parts by weight of resin, graphene is 2 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR of the resin component is tested. B =4.4g / 10min.
[0082] (3) Preparation of composite films:
[0083] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.
[0084] Example 3
[0085] This example is used to illustrate the preparation of the antistatic composite film provided by the present invention.
[0086] An antistatic polypropylene composite film was prepared according to Example 1, except that the conductive fillers were multi-walled carbon nanotubes and conductive carbon black. Based on 100 parts by weight of the resin, the multi-walled carbon nanotubes were 1 part by weight, and the conductive carbon black was 1 part by weight.
[0087] Example 4
[0088] This example is used to illustrate the preparation of the antistatic composite film provided by the present invention.
[0089] (1) Preparation of polypropylene composition A:
[0090] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =3.3g / 10min.
[0091] (2) Preparation of polypropylene composition B:
[0092] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 75 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 1:2. The pellets of polypropylene composition B are obtained, and the melt mass flow rate MFR of the resin component is tested. B =5.5g / 10min.
[0093] (3) Preparation of composite films:
[0094] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0095] Example 5
[0096] A polypropylene film was prepared according to the method of Example 2. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. Wb:Wy is 5:4. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.3g / 10min.
[0097] Example 6
[0098] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 99 parts by weight, and the mass fraction Wb of component b is 1 part by weight. Wb:Wy is 1:5. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.2g / 10min.
[0099] Example 7
[0100] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 25 parts by weight, and the mass fraction Wz of component z is 25 parts by weight. Wb:Wy is 4:5. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin components thereof was tested. B=4.0g / 10min.
[0101] Example 8
[0102] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 4:1. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin components thereof was tested. B =8.2g / 10min.
[0103] Example 9
[0104] A polypropylene film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition A, the mass fraction Wa of component a was 100 parts by weight, and component b was not added. Granules of the polypropylene composition A were obtained.
[0105] Comparative Example 1
[0106] A composite film was prepared according to the method of Example 1, except that the polypropylene composition B did not contain a conductive filler.
[0107] Comparative Example 2
[0108] A composite film was prepared according to the method of Example 1, except that the polypropylene composition B only contained component x and multi-walled carbon nanotubes as a conductive filler.
[0109] Comparative Example 3
[0110] A composite film was prepared according to the method of Example 1, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 50 μm.
[0111] Table 1
[0112]
[0113]
[0114] It can be concluded from the results of the examples in Table 1 that the antistatic polypropylene composite film provided by the present invention has good impact resistance, tensile properties, antistatic properties and heat sealing strength. The longitudinal (MD) tensile strength of the film of the present invention is ≥45MPa, preferably ≥52MPa. The pendulum impact strength is ≥0.6J, preferably ≥1.5J. The heat sealing strength at 150°C is ≥15N / 15mm, preferably ≥18N / 15mm. The surface resistivity is 10 2 -10 8 Ω, preferably 10 2 -10 4Ω. The composite film after adding conductive fillers not only meets the antistatic use requirements, but also has good mechanical properties, which can meet the application requirements of high-end packaging fields such as battery packaging materials, electronic product packaging materials, powder packaging materials or high-end food packaging materials. From the comparative examples, it can be seen that it is difficult to achieve a balance of various properties by changing the composition ratio of the film layer, and during extrusion casting, the film surface is unstable and it is difficult to obtain a film with uniform thickness.
[0115] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0116] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. An antistatic polypropylene composite film, characterized in that: The polypropylene composite film is composed of at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a and a polyolefin elastomer b, the polypropylene composition B comprises a resin component and a conductive filler, and the resin component comprises random polypropylene x, polyolefin elastomer y and propylene impact copolymer z; Based on the total weight of the polypropylene composition A, the polypropylene composition A includes 70-95wt% of polypropylene a and 5-30wt% of polyolefin elastomer b; in the polypropylene composition B, based on 100 parts by weight of the resin component, the content of the conductive filler is 0.1-10 parts by weight, and the resin component includes 50-90wt% of random polypropylene x, 5-35wt% of polyolefin elastomer y, and 2-30wt% of propylene impact copolymer z; Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 6:1-1:6; The propylene impact copolymer z is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer z, the ethylene content of the propylene impact copolymer z is 1-12wt%; the polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an alpha olefin; When the polypropylene composite film has a structure of three or more layers, the film layer B is the surface layer.
2. The antistatic polypropylene composite film according to claim 1, characterized in that: The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥45MPa; pendulum impact strength ≥0.6J; heat sealing strength at 150°C ≥15N / 15mm; surface resistivity ≥10 2 -10 8 Ω.
3. The antistatic polypropylene composite film according to claim 2, characterized in that: The longitudinal tensile strength is ≥52MPa.
4. The antistatic polypropylene composite film according to claim 2, characterized in that: The pendulum impact strength is ≥1.5J.
5. The antistatic polypropylene composite film according to claim 2, characterized in that: The heat sealing strength at 150° C. is ≥18N / 15mm.
6. The antistatic polypropylene composite film according to claim 2, characterized in that: The surface resistivity is 10 2 -10 4 Ω.
7. The antistatic polypropylene composite film according to claim 1, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min.
8. The antistatic polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 3-8 g / 10 min.
9. The antistatic polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 4-8 g / 10 min.
10. The antistatic polypropylene composite film according to claim 1, characterized in that: The polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.
11. The antistatic polypropylene composite film according to claim 10, characterized in that: The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.
0.
12. The antistatic polypropylene composite film according to claim 10, characterized in that: The propylene impact copolymer is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer, the ethylene content of the propylene impact copolymer is 1-12wt%; the content of the copolymerized part containing ethylene units in the propylene impact copolymer is 3-15wt%; the melt mass flow rate of the propylene impact copolymer at 230°C and a load of 2.16kg is 1-10g / 10min.
13. The antistatic polypropylene composite film according to claim 1, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer z has a content of 3-15wt%; The propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.
14. The antistatic polypropylene composite film according to claim 1, characterized in that: The alpha olefin is C3-C 12 of alpha olefins.
15. The antistatic polypropylene composite film according to claim 14, characterized in that: The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
16. The antistatic polypropylene composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.
17. The antistatic polypropylene composite film according to claim 16, characterized in that: The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.
18. The antistatic polypropylene composite film according to claim 1, characterized in that: The conductive filler is selected from at least one of carbon black conductive fillers, graphite conductive fillers, carbon nanotube conductive fillers, carbon fiber conductive fillers, conductive metal particles, conductive metal fibers, fillers coated with conductive metals, and metal oxides.
19. The antistatic polypropylene composite film according to claim 18, characterized in that: The carbon black conductive filler is at least one of acetylene black, superconducting carbon black and special conductive carbon black; the graphite conductive filler is at least one of natural graphite, expandable graphite, expanded graphite and graphene; the carbon nanotube conductive filler is single-walled carbon nanotubes and / or multi-walled carbon nanotubes that are not surface-modified or surface-modified; the conductive metals in the conductive metal particles and conductive metal fibers are each independently at least one of silver, aluminum, copper, iron, nickel and stainless steel; the filler coated with conductive metal is selected from at least one of lead-plated, nickel-plated, silver-plated glass balls, glass fibers and mica sheets; the metal oxide is at least one of titanium oxide, zinc oxide, tin oxide, indium oxide and cadmium oxide.
20. The antistatic polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 80-95 wt% of the polypropylene a and 5-20 wt% of the polyolefin elastomer b.
21. The antistatic polypropylene composite film according to claim 1, characterized in that: In the polypropylene composition B, based on 100 parts by weight of the resin component, the content of the conductive filler is 0.5-4.5 parts by weight, and the resin component includes 60-85wt% of random polypropylene x, 5-20wt% of polyolefin elastomer y, and 5-20wt% of propylene impact copolymer z.
22. The antistatic polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 4:1-1:
4.
23. The antistatic polypropylene composite film according to any one of claims 1 to 22, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:
1.
24. The antistatic polypropylene composite film according to claim 23, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:3-1:
1.
25. The antistatic polypropylene composite film according to any one of claims 1 to 22, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.
26. The antistatic polypropylene composite film according to claim 25, characterized in that: The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.
27. The antistatic polypropylene composite film according to claim 25, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.
28. The antistatic polypropylene composite film according to claim 27, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.
29. The antistatic polypropylene composite film according to claim 25, characterized in that: The lubricant is a PEG lubricant and / or a monoglyceride lubricant.
30. The antistatic polypropylene composite film according to claim 25, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.
31. The antistatic polypropylene composite film according to claim 30, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.
32. The antistatic polypropylene composite film according to any one of claims 1 to 22, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.
33. The antistatic polypropylene composite film according to claim 32, characterized in that: The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant and an anti-sticking agent.
34. The antistatic polypropylene composite film according to claim 32, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.
35. The antistatic polypropylene composite film according to claim 34, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.
36. The method for preparing the antistatic polypropylene composite film according to any one of claims 1 to 35, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.
37. The preparation method according to claim 36, characterized in that: The stretching is bidirectional stretching.
38. Use of the antistatic polypropylene composite film according to any one of claims 1 to 35 in the field of packaging materials.
39. The use according to claim 38, characterized in that The packaging is battery packaging, electronic product packaging, industrial powder packaging or food packaging.