Low-haze, high-impact, colored, heat-sealable polypropylene composite film, preparation method and application thereof

By using a composition with a double-layer or multi-layer structure in a polypropylene film, combining resin, colorant and impact copolymer, the lack of optical and impact resistance of the polypropylene film is solved, and efficient heat sealing and impact resistance are achieved. Performance, suitable for high-end packaging materials.

CN115991040BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111223372.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-11-19
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

The existing polypropylene films are difficult to have good optical and impact resistance at the same time, and the heat sealing performance is insufficient at low heat sealing temperatures, making it difficult to meet the multiple needs of packaging materials.

Method used

Polypropylene composite film with a double-layer or multi-layer structure, by combining polypropylene composition A and polypropylene composition B, respectively, includes resin components, colorants, random polypropylene, polyolefin elastomer and propylene impact resistance. The copolymer is prepared by extrusion casting method to ensure the uniformity and mechanical properties of the material.

Benefits of technology

The film has achieved high impact resistance, good optical properties and good heat sealing strength, longitudinal tensile strength ≥35MPa, pendulum impact strength ≥0.4J, heat sealing strength at 150℃ ≥13N/15mm, film haze ≤6% , suitable for high-end packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003313421290000141
    Figure BDA0003313421290000141
  • Figure BDA0003313421290000151
    Figure BDA0003313421290000151
Patent Text Reader

Abstract

The present invention belongs to the field of films, and relates to a low-haze, high-impact, colored, heat-sealable polypropylene composite film, and a preparation method and application thereof. The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises a resin component and a colorant, the resin component comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, polyolefin elastomer y, and propylene impact copolymer z. The antistatic composite film of the present invention has good impact resistance, tensile properties, and antistatic properties at the same time, and has good heat sealing strength at a relatively low heat sealing temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of films, and in particular relates to a low-fog, high-impact, colored, heat-sealable polypropylene composite film, and a preparation method and application thereof. Background Art

[0002] Polypropylene film can usually be made by methods such as casting and biaxial stretching, but polypropylene film made from homopolymer polypropylene raw materials usually has low impact strength. Polypropylene film is often used for packaging purposes, which requires the film to have high impact performance. At the same time, for the visualization and aesthetics of the contents, the film is also expected to have good optical properties. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomers can be added to polypropylene, but the films prepared by the above methods usually have high haze and poor optical properties such as transparency. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.

[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3. The elastomer provides good impact resistance. However, this method has the problem of difficulty in uniform dispersion when the elastomer content is high, and it is still difficult to obtain a film with good optical properties. In addition, the amount of elastomer added will be limited, because when the amount added reaches a certain level, phase separation will occur, thereby limiting the further improvement of impact performance. Moreover, when the film is used for packaging purposes, it is usually hoped that it has good heat sealing performance and bright color appearance at a lower heat sealing temperature. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good optical properties and impact resistance at the same time, and to provide a low-haze high-impact colored heat-seal film and a preparation method thereof. The polypropylene film of the present invention has good impact resistance, optical properties and tensile properties at the same time, has the expected color, and has good heat-seal strength at a relatively low heat-seal temperature.

[0005] The first aspect of the present invention provides a low-haze, high-impact, colored, heat-seal polypropylene composite film, the polypropylene composite film comprising at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises a resin component and a colorant, the resin component comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises a random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z.

[0006] The second aspect of the present invention provides a method for preparing the above-mentioned low-haze, high-impact, colored, heat-sealable polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0007] The third aspect of the present invention provides the use of the low-haze, high-impact, colored, heat-seal polypropylene composite film in the field of packaging materials.

[0008] The antistatic composite film of the present invention has good impact resistance, tensile properties and antistatic properties, and has good heat sealing strength at a relatively low heat sealing temperature. The longitudinal (MD) tensile strength of the film is ≥35MPa, preferably ≥48MPa; the pendulum impact strength is ≥0.4J, preferably ≥1.3J; the heat sealing strength at 150°C is ≥13N / 15mm, preferably ≥17N / 15mm; the film haze is ≤6%, preferably ≤2.5%.

[0009] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0010] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0011] The present invention provides a low-haze, high-impact, colored, heat-sealable polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises a resin component and a colorant, the resin component comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, polyolefin elastomer y and a propylene impact copolymer z.

[0012] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥35MPa, preferably longitudinal (MD) tensile strength ≥48MPa; pendulum impact strength ≥0.4J, preferably pendulum impact strength ≥1.3J; heat sealing strength at 150°C ≥13N / 15mm, preferably heat sealing strength at 150°C ≥17N / 15mm; film haze ≤6%, preferably film haze ≤2.5%.

[0013] According to some embodiments of the present invention, the polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.

[0014] Preferably, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available, such as homopolypropylene with a grade of PPH-FA03 from Qingdao Refining and Chemical and homopolypropylene with a grade of FC801 from Shanghai Petrochemical. Alternatively, it can be prepared by conventional methods in the art.

[0015] According to the present invention, the propylene impact copolymer is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymer part containing ethylene units, preferably selected from an ethylene-propylene copolymer part and an ethylene-butene copolymer part.

[0016] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.

[0017] Based on the total weight of the propylene impact copolymer z, the content of the copolymerized part containing ethylene units in the propylene impact copolymer z is preferably 3-15wt%. 13 C NMR determination.

[0018] The ethylene content of the propylene impact copolymer z is preferably 1-12 wt%, based on the total weight of the propylene impact copolymer z.

[0019] The propylene impact copolymer z preferably has a melt mass flow rate of 1 to 10 g / 10 min at 230° C. and a load of 2.16 kg.

[0020] The propylene impact copolymer may have a block structure or include a propylene block copolymer.

[0021] The optional propylene impact copolymer of the polypropylene a and the propylene impact copolymer z may be the same or different, preferably satisfying the above conditions.

[0022] Propylene impact copolymers meeting the above characteristics are commercially available, such as propylene impact copolymers with the brand name EP200K from Sinopec, propylene impact copolymers with the brand name PPB-M02D from Maoming Petrochemical, and propylene impact copolymers with the brand name M180R from Shanghai Petrochemical. Alternatively, they can be prepared by conventional methods in the art.

[0023] According to some embodiments of the present invention, the polyolefin elastomer b is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0024] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0025] The polyolefin elastomers meeting the above characteristics are commercially available, for example, polyolefin elastomers with the trademark of Exxon 6102, polyolefin elastomers with the trademark of Exxon EXACT 3139, and polyolefin elastomers with the trademark of Mitsui DF640. Alternatively, they can be prepared by conventional methods in the art.

[0026] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.

[0027] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.

[0028] Random polypropylene meeting the above characteristics is commercially available, such as Yanshan Petrochemical's F5006 random polypropylene and Shanghai Petrochemical's F800EPS random polypropylene, or can be prepared by conventional methods in the art.

[0029] According to some embodiments of the present invention, the colorant may be a conventional choice in the art, including but not limited to at least one of azo pigments, phthalocyanine pigments, heterocyclic pigments, lake pigments, dyes, fluorescent brighteners and fluorescent pigments. The above colorants are all commercially available.

[0030] According to some embodiments of the present invention, in the polypropylene composition A, the content of the colorant is 0.1-1 parts by weight, based on 100 parts by weight of the resin component, and the resin component includes 70-100 wt% of polypropylene a and 0-30 wt% of polyolefin elastomer b.

[0031] According to a preferred embodiment of the present invention, in the polypropylene composition A, based on 100 parts by weight of the resin component, the content of the colorant is 0.3-0.8 parts by weight, and the resin component includes 80-95wt% of polypropylene a and 5-20wt% of polyolefin elastomer b.

[0032] In the resin component of the present invention, the elastomer or propylene impact copolymer in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular chain segments of the homopolymer phase of homopolypropylene and propylene impact copolymer are relatively regular, crystallization and orientation occur during the film preparation process, providing good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the rubber phase can be evenly distributed in the film, and the size of the rubber phase can meet the requirements of the refractive index, so that a film with good optical properties can be obtained, so that the film has good impact performance and optical properties at the same time; at the same time, under this ratio, the composition also contains enough homopolymer phase, so that the film has good mechanical properties.

[0033] According to some embodiments of the present invention, the polypropylene composition B comprises 50-90 wt% of random polypropylene x, 5-30 wt% of polyolefin elastomer y and 2-30 wt% of propylene impact copolymer z.

[0034] According to a preferred embodiment of the present invention, the polypropylene composition B comprises 60-85 wt% of random polypropylene x, 5-20 wt% of polyolefin elastomer y and 5-20 wt% of propylene impact copolymer z.

[0035] According to the research of the present inventors, when the polypropylene composition B adopts this ratio and the surface layer in the composite film is made of the polypropylene composition B, the impact resistance of the film can be greatly improved, and the optical properties can be further improved, and the film can also have good heat sealing properties.

[0036] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:6, for example, it can be 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 and any value therebetween.

[0037] According to a preferred embodiment of the present invention, the ratio of Wb to Wy is 4:1-1:4.

[0038] According to the research conducted by the present inventors, when a double-layer or multi-layer film is co-extruded, when the ratio of Wb to Wy is within the range described in the present invention, the impact resistance and optical properties of the film can be further improved, and at the same time the extrusion process will be smoother.

[0039] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min.

[0040] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min.

[0041] When the melt mass flow rates of the resin components of the polypropylene composition A and the polypropylene composition B are within the above ranges, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity, mechanical properties and optical properties.

[0042] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may be the same as the resin component of the film layer A or the film layer B, or may be different from the resin component of the film layer A or the film layer B, or may be a mixture of a polypropylene composition A and a polypropylene composition B. When the polypropylene composite film is a three-layer or more structure, the film layer B is preferably used as a surface layer, such as a three-layer film including a film layer A, a film layer B, and a film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.

[0043] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.

[0044] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:2-1:1. Under this ratio, the composite film has good mechanical properties.

[0045] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.

[0046] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.

[0047] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.

[0048] According to the present invention, in order to improve other properties (such as stability, etc.) of the composite film, the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a filler, a lubricant, and an anti-adhesive agent (anti-adhesive agent). The specific type of the film-forming aid can be a conventional choice in the art, and will not be repeated here.

[0049] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.

[0050] According to some embodiments of the present invention, the polypropylene composition A further comprises a dispersant. The dispersant can improve the processability and uniformity between the resin component and the colorant of the polypropylene composition A, and its type, usage and dosage can be conventionally selected in the art, for example, the dispersant can be a low molecular weight polyethylene wax, and the weight content of the dispersant can be 20-30wt% of the colorant.

[0051] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0052] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.

[0053] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.

[0054] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.

[0055] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.

[0056] The composite film of the invention has good impact resistance and optical properties, and the film has good uniformity.

[0057] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as high-end packaging fields that require both high impact resistance and optical properties of the film, including but not limited to battery packaging, electronic product packaging or high-end food packaging.

[0058] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.

[0059] In the following examples and comparative examples:

[0060] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.

[0061] The properties of the polypropylene composition and polypropylene composite film were tested according to the following method, and the film test results are shown in Table 1:

[0062] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.

[0063] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.

[0064] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.

[0065] (4) Film haze: measured according to the method specified in GB / T 2410-2008.

[0066] (5) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.

[0067] (6) Isoregularity: Pass 13C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.

[0068] (7) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.

[0069] Example 1

[0070] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0071] (1) Preparation of polypropylene composition A:

[0072] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is polyolefin elastomer with the brand name 6102, purchased from Exxon, and is an ethylene-propylene copolymer with an ethylene structural unit content of 16 wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then add lubricant (the lubricant is PEG lubricant produced by Clariant, Switzerland, with a molecular weight of 10,000, and the amount of lubricant added is 0.1 parts by weight based on the sum of the mass of the above-mentioned component a and component b as 100 parts by weight); add colorant light-fast brilliant red BBS (color index CIPR48:3, commercially available), the amount of colorant added is 0.5 parts by weight based on the sum of the mass of the above-mentioned component a and component b as 100 parts by weight; add dispersant (low molecular weight polyethylene wax, commercially available), the amount of dispersant added is 25 parts by weight based on 100 parts by weight of the colorant. Then add the mixture to a high-speed stirrer and mix evenly, then add the mixed material to the feeder of a twin-screw extruder manufactured by W&P, the material enters the twin screw through the feeder, the temperature of the screw is maintained between 160-230°C during the processing, the screw is melt-mixed evenly, extruded, granulated and dried to obtain polypropylene composition A pellets, and the melt mass flow rate MFR of its resin component is tested. A =3.5g / 10min.

[0073] (2) Preparation of polypropylene composition B:

[0074] Component x is a random polypropylene with a grade of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2g / 10min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%; component z is a propylene impact copolymer with a grade of EP200K, purchased from China Sands Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 13wt%, and a melt mass flow rate of 3.2g / 10min. The components prepared above are weighed and mixed according to the proportions, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. Wb:Wy is 4:1. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =4.7g / 10min.

[0075] (3) Preparation of composite films:

[0076] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.

[0077] Example 2

[0078] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0079] (1) Preparation of polypropylene composition A:

[0080] Component a is homopolypropylene with the brand name FC801, purchased from Shanghai Petrochemical, with a melt mass flow rate of 7.8 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.8; component b is a polyolefin elastomer with the brand name EXACT3139, purchased from Exxon, and is an ethylene-1-octene copolymer with an octene structural unit content of 14 wt%. The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 85 parts by weight, and the mass fraction Wb of component b is 15 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant, Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the mass of the above-mentioned component a and component b being 100 parts by weight); a colorant phthalocyanine green (color index CIPG7, commercially available) is added, and the amount of the colorant added is 0.8 parts by weight based on the sum of the mass of the above-mentioned component a and component b being 100 parts by weight; a dispersant (low molecular weight polyethylene wax, commercially available) is added, and the amount of the dispersant added is 20 parts by weight based on 100 parts by weight of the colorant. After that, the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. After the screw is melt-mixed, extruded, granulated and dried, a pellet of polypropylene composition A is obtained. The melt mass flow rate MFR of its resin component is tested. A =7.9g / 10min.

[0081] (2) Preparation of polypropylene composition B:

[0082] Component x is a random polypropylene with the brand name F800EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 8.2g / 10min; component y is a polyolefin elastomer with the brand name EXACT3139, purchased from Exxon, which is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%; component z is a propylene impact copolymer with the brand name PPB-M02D, purchased from Maoming Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 10wt%, and a melt mass flow rate of 1.5g / 10min. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 3:2. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =7.4g / 10min.

[0083] (3) Preparation of composite films:

[0084] The preparation process is the same as step (3) of Example 1.

[0085] Example 3

[0086] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wz of component z is 40 parts by weight. Wb:Wy is 2:1. And the colorant in the polypropylene composition A is permanent violet (color index CIPV23). The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR thereof was tested. B =4.8g / 10min.

[0087] Example 4

[0088] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, component a is a propylene impact copolymer with the grade M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; component b is a polyolefin elastomer with the grade DF640, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%. The mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Wb:Wy is 1:1. Polypropylene composition A pellets were obtained, and the melt mass flow rate MFR of its resin component was tested. A =3.1g / 10min.

[0089] Step (3) is the same as in Example 1. The film thickness is 50 μm, wherein the thickness ratio of film layer B to film layer A is 1:1.

[0090] Example 5

[0091] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. Wb:Wy is 5:1. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR of the resin component was tested. A =3.1g / 10min.

[0092] Example 6

[0093] A polypropylene composite film was prepared according to the method of Example 4. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 99 parts by weight, and the mass fraction Wb of component b is 1 part by weight. Wb:Wy is 1:5. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR of the resin component was tested. A =3.2g / 10min.

[0094] Example 7

[0095] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 4:1. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR thereof was tested. B =8.2g / 10min.

[0096] Example 8

[0097] A polypropylene composite film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition A, the mass fraction Wx of component a was 100 parts by weight, and component b was not added.

[0098] Comparative Example 1

[0099] A polypropylene composite film was prepared according to the method of Example 1. The difference was that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 50 μm.

[0100] Comparative Example 2

[0101] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition A did not contain a colorant, and only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 50 μm.

[0102] Comparative Example 3

[0103] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x and component z, wherein the mass fraction Wx of component x was 70 parts by weight, and the mass fraction Wz of component z was 30 parts by weight.

[0104] Table 1

[0105]

[0106]

[0107] It can be concluded from the results of the embodiments in Table 1 that the polypropylene composite film provided by the present invention has bright colors and good impact resistance, optical properties and tensile properties, and has good heat sealing strength. The longitudinal (MD) tensile strength of the film of the present invention is ≥35MPa, the film haze is ≤6%, the pendulum impact strength is ≥0.4J, and the heat sealing strength at 150°C is ≥13N / 15mm. It can be seen from the preferred embodiments that the longitudinal (MD) tensile strength of the film of the present invention is ≥48MPa, the film haze is ≤2.5%, the pendulum impact strength is ≥1.3J, and the heat sealing strength at 150°C is ≥17N / 15mm. It can be seen from the comparative examples that it is difficult to achieve a balance of various properties by only using a single-layer film or changing the composition ratio of the film layer, and during extrusion casting, the film surface is unstable, and it is difficult to obtain a film with uniform thickness.

[0108] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0109] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A low haze, high impact resistant, colored, heat-sealable polypropylene composite film, characterized in that: The polypropylene composite film is composed of at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises a resin component and a colorant, the resin component comprises polypropylene a and a polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, polyolefin elastomer y and propylene impact copolymer z; In the polypropylene composition A, based on 100 parts by weight of the resin component, the content of the colorant is 0.1-1 parts by weight, and the resin component comprises 70-95 wt% of polypropylene a and 5-30 wt% of polyolefin elastomer b; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 50-90 wt% of random polypropylene x, 5-30 wt% of polyolefin elastomer y and 2-40 wt% of propylene impact copolymer z; Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 6:1-1:6; The propylene impact copolymer z is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer z, the ethylene content of the propylene impact copolymer z is 1-12wt%; the polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and alpha olefin.

2. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 1, characterized in that: The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥35 MPa; pendulum impact strength ≥0.4 J; heat sealing strength at 150° C. ≥13 N / 15 mm; and film haze ≤6%.

3. The low haze and high impact colored heat-seal polypropylene composite film according to claim 2, characterized in that: The longitudinal tensile strength is ≥48MPa.

4. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 2, characterized in that: The pendulum impact strength is ≥1.3J.

5. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 2, characterized in that: The heat sealing strength at 150° C. is ≥17N / 15mm.

6. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 2, characterized in that: The haze of the film is ≤2.5%.

7. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min.

8. The low-haze, high-impact colored heat-seal polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition A is 3-8 g / 10 min.

9. The low haze and high impact colored heat-seal polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 4-8 g / 10 min.

10. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: The polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.

11. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 10, characterized in that: The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.

0.

12. The low haze and high impact colored heat-seal polypropylene composite film according to claim 10, characterized in that: The propylene impact copolymer is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer, the ethylene content of the propylene impact copolymer is 1-12wt%; the content of the copolymerized part containing ethylene units in the propylene impact copolymer is 3-15wt%; the melt mass flow rate of the propylene impact copolymer at 230°C and a load of 2.16kg is 1-10g / 10min.

13. The low haze and high impact resistant colored heat seal polypropylene composite film according to claim 1, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer z has a content of 3-15wt%; The propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

14. The low haze and high impact resistant colored heat seal polypropylene composite film according to claim 1, characterized in that: The alpha olefin is C3-C 12 of alpha olefins.

15. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 14, characterized in that: The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

16. The low haze and high impact resistant colored heat seal polypropylene composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.

17. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 16, characterized in that: The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.

18. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: The colorant is selected from at least one of azo pigments, phthalocyanine pigments, heterocyclic pigments, lake pigments, dyes, fluorescent brighteners and fluorescent pigments.

19. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: In the polypropylene composition A, based on 100 parts by weight of the resin component, the content of the colorant is 0.3-0.8 parts by weight, and the resin component comprises 80-95 wt% of polypropylene a and 5-20 wt% of polyolefin elastomer b.

20. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 60-85 wt% of random polypropylene x, 5-20 wt% of polyolefin elastomer y and 5-20 wt% of propylene impact copolymer z.

21. The low haze and high impact colored heat-seal polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 4:1-1:

4.

22. The low haze, high impact resistant, colored, heat-sealable polypropylene composite film according to any one of claims 1 to 21, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:

1.

23. The low haze and high impact resistant colored heat-seal polypropylene composite film according to claim 22, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:2-1:

1.

24. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to any one of claims 1 to 21, characterized in that: When the polypropylene composite film has a structure of three or more layers, the film layer B is the surface layer.

25. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to any one of claims 1 to 21, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.

26. The low haze and high impact colored heat-seal polypropylene composite film according to claim 25, characterized in that: The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.

27. The low haze and high impact colored heat-seal polypropylene composite film according to claim 25, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.

28. The low haze and high impact colored heat-seal polypropylene composite film according to claim 27, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.

29. The low haze and high impact colored heat-seal polypropylene composite film according to claim 25, characterized in that: The lubricant is a PEG lubricant and / or a monoglyceride lubricant.

30. The low haze and high impact colored heat-seal polypropylene composite film according to claim 25, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.

31. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to claim 30, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.

32. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to any one of claims 1 to 21, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.

33. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to claim 32, characterized in that: The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a filler, a lubricant and an anti-sticking agent.

34. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to claim 32, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.

35. The low haze and high impact colored heat-seal polypropylene composite film according to claim 34, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.

36. The low haze, high impact resistant, colored, heat-sealable polypropylene composite film according to any one of claims 1 to 21, characterized in that: The polypropylene composition A further comprises a dispersant, and the weight content of the dispersant is 20-30 wt % of the colorant.

37. The low haze, high impact resistant, colored heat-seal polypropylene composite film according to claim 36, characterized in that: The dispersant is low molecular weight polyethylene wax.

38. The method for preparing the low-haze, high-impact, colored, heat-sealable polypropylene composite film according to any one of claims 1 to 37, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.

39. The preparation method according to claim 38, characterized in that: The stretching is bidirectional stretching.

40. Use of the low-haze, high-impact, colored, heat-sealable polypropylene composite film according to any one of claims 1 to 37 in the field of packaging materials.

41. The use according to claim 40, characterized in that The packaging is battery packaging, electronic product packaging or food packaging.