Electromagnetic shielding polypropylene composite film and its preparation method and application

By using a double-layer or multi-layer structure electromagnetic shielding polypropylene composite film in polypropylene film, combining homopolypolypropylene and electromagnetic shielding filler, the insufficient heat sealing strength of polypropylene films when improving impact resistance and electromagnetic shielding performance is solved. The problem is that high-performance electromagnetic shielding and mechanical properties are achieved.

CN115991041BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111223377.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-11-19
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

While improving impact resistance and electromagnetic shielding performance, existing polypropylene films are difficult to maintain good heat seal strength at low heat sealing temperatures, and the addition of electromagnetic shielding fillers will lead to deterioration of material properties.

Method used

Electromagnetic shielded polypropylene composite film with a double-layer or multi-layer structure, by combining polypropylene composition A and polypropylene composition B, wherein polypropylene composition A contains homopolymer and propylene impact copolymer, Propylene composition B contains random polypropylene, polyolefin elastomer and electromagnetic shielding filler. The film is prepared by extrusion casting method to ensure the uniformity and mechanical properties of the material.

Benefits of technology

The film has achieved high heat seal strength, good impact resistance and electromagnetic shielding performance under low heat sealing temperature. The longitudinal tensile strength is ≥28MPa, the pendulum impact strength is ≥0.4J, and the heat seal strength at 150℃ is ≥12N/15mm. , electromagnetic shielding performance ≥25dB.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003313422490000151
    Figure BDA0003313422490000151
Patent Text Reader

Abstract

The present invention belongs to the field of films, and relates to an electromagnetic shielding polypropylene composite film, a preparation method thereof, and an application thereof. The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises a resin component and an electromagnetic shielding filler, wherein the resin component comprises random polypropylene x, polyolefin elastomer y, and propylene impact copolymer z. The electromagnetic shielding composite film of the present invention has good impact resistance, tensile properties, and electromagnetic shielding properties at the same time, and has good heat sealing strength at a relatively low heat sealing temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of films, and in particular relates to an electromagnetic shielding polypropylene composite film and a preparation method and application thereof. Background Art

[0002] Polypropylene film can usually be made by casting and biaxial stretching, but the impact strength of polypropylene film made from homopolymer polypropylene raw materials is usually low. To improve the impact performance of polypropylene film, block impact polypropylene can be used to make the film, or polyolefin elastomer can be added to polypropylene, but the film prepared by the above methods usually has a high haze. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.

[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3. The elastomer provides good impact resistance. However, this method has the problem of difficulty in uniform dispersion when the elastomer content is high, and the amount of elastomer added will be limited, because when the amount added reaches a certain level, phase separation will occur, thereby limiting the further improvement of impact performance. Moreover, when the film is used for packaging purposes, it is usually hoped that it has good heat sealing performance at a lower heat sealing temperature.

[0004] With the rapid development of the electronic information industry, the number of electronic products that generate electromagnetic interference has increased dramatically, and electromagnetic interference has become a public nuisance; at the same time, precision electronic equipment and components are also easily damaged by electromagnetic interference. Electromagnetic shielding materials have been widely valued and applied as an effective means of electromagnetic protection. At present, polymer-based electromagnetic shielding materials have the advantages of one-time molding and processing and low prices, and are an important development direction of electromagnetic shielding materials. Electromagnetic shielding films mainly use PET, PP, etc., and achieve electromagnetic shielding by adding electromagnetic shielding fillers, etc., but metal fillers will greatly deteriorate the performance of the film. Therefore, it is necessary to develop a high-performance electromagnetic shielding film to reduce the deterioration of material performance after adding electromagnetic shielding fillers. Summary of the invention

[0005] The purpose of the present invention is to provide an electromagnetic shielding polypropylene composite film and a preparation method thereof. The electromagnetic shielding film has good impact resistance, tensile properties, electromagnetic shielding properties, and good heat sealing strength at a relatively low heat sealing temperature.

[0006] The first aspect of the present invention provides an electromagnetic shielding polypropylene composite film, which includes at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A includes polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B includes a resin component and an electromagnetic shielding filler, and the resin component includes a random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z.

[0007] The second aspect of the present invention provides a method for preparing the electromagnetic shielding polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0008] The third aspect of the present invention provides application of the electromagnetic shielding polypropylene composite film in the field of packaging materials.

[0009] The electromagnetic shielding composite film of the present invention has good impact resistance, tensile properties and electromagnetic shielding properties, and has good heat sealing strength at a relatively low heat sealing temperature. The longitudinal (MD) tensile strength of the film is ≥28MPa, preferably ≥35MPa; the pendulum impact strength is ≥0.4J, preferably ≥0.9J; the heat sealing strength at 150°C is ≥12N / 15mm, preferably ≥14N / 15mm; the electromagnetic shielding effectiveness is ≥25dB, preferably ≥28dB.

[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0012] The present invention provides an electromagnetic shielding polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises a resin component and an electromagnetic shielding filler, and the resin component comprises a random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z.

[0013] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥28 MPa, preferably longitudinal tensile strength ≥35 MPa; pendulum impact strength ≥0.4 J, preferably pendulum impact strength ≥0.9 J; heat sealing strength at 150°C ≥12 N / 15 mm, preferably heat sealing strength at 150°C ≥14 N / 15 mm; electromagnetic shielding effectiveness ≥25 dB, preferably electromagnetic shielding effectiveness ≥28 dB.

[0014] According to some embodiments of the present invention, the polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.

[0015] Preferably, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available, such as the homopolypropylene with the grade PPH-FA03 of Qingdao Refining and Chemical Co., Ltd. Alternatively, it can be prepared by conventional methods in the art.

[0016] According to the present invention, the propylene impact copolymer is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymer part containing ethylene units, preferably selected from an ethylene-propylene copolymer part and an ethylene-butene copolymer part.

[0017] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.

[0018] Based on the total weight of the propylene impact copolymer z, the content of the copolymerized part containing ethylene units in the propylene impact copolymer z is preferably 3-15wt%. 13 C NMR determination.

[0019] The ethylene content of the propylene impact copolymer z is preferably 1-12 wt%, based on the total weight of the propylene impact copolymer z.

[0020] The propylene impact copolymer z preferably has a melt mass flow rate of 1 to 10 g / 10 min at 230° C. and a load of 2.16 kg.

[0021] The propylene impact copolymer may have a block structure or include a propylene block copolymer.

[0022] The optional propylene impact copolymer of the polypropylene a and the propylene impact copolymer z may be the same or different, preferably satisfying the above conditions.

[0023] The propylene impact copolymers meeting the above characteristics are commercially available, such as the propylene impact copolymers with the brand name EP200K of Sinopec and the propylene impact copolymers with the brand name M180R of Shanghai Petrochemical, or can be prepared by conventional methods in the art.

[0024] According to some embodiments of the present invention, the polyolefin elastomer b is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0025] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0026] The polyolefin elastomer meeting the above characteristics is commercially available, for example, the polyolefin elastomer with the brand number 6102 from Exxon and the polyolefin elastomer with the brand number DF640 from Mitsui, or can be prepared by conventional methods in the art.

[0027] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.

[0028] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.

[0029] Random polypropylene meeting the above characteristics is commercially available, such as Yanshan Petrochemical's F5006 random polypropylene and Shanghai Petrochemical's F500EPS random polypropylene, or can be prepared by conventional methods in the art.

[0030] According to some embodiments of the present invention, the electromagnetic shielding filler is a conductive metal filler and / or a carbon material. The conductive metal filler is preferably conductive metal particles and / or conductive metal fibers. Further preferably, the metals in the conductive metal particles and conductive metal fibers are each independently selected from one or more of silver, aluminum, copper, iron, nickel and stainless steel. The carbon material is preferably one or more of carbon black, graphite, graphene and carbon nanotubes.

[0031] According to some embodiments of the present invention, the polypropylene composition A comprises 70-100 wt% of polypropylene a and 0-30 wt% of polyolefin elastomer b.

[0032] According to a preferred embodiment of the present invention, the polypropylene composition A comprises 80-95 wt% of polypropylene a and 5-20 wt% of polyolefin elastomer b.

[0033] In the resin component of the present invention, the elastomer or propylene impact copolymer in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular segments of the homopolymer phase of homopolypropylene and propylene impact copolymer are relatively regular, crystallization and orientation occur during the film preparation process, providing good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the rubber phase can be evenly distributed in the film so that the film has good impact performance; at the same time, under this ratio, the composition also contains enough homopolymer phase, so that the film has good mechanical properties.

[0034] According to some embodiments of the present invention, in the polypropylene composition B, based on the weight of the resin component as 100 parts by weight, the content of the electromagnetic shielding filler is 5-30 parts by weight, specifically 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 18 parts by weight, 20 parts by weight, 25 parts by weight, and 28 parts by weight, and the resin component includes 50-90wt% of random polypropylene x, 5-30wt% of polyolefin elastomer y, and 2-30wt% of propylene impact copolymer z.

[0035] According to a preferred embodiment of the present invention, based on 100 parts by weight of the resin component, the content of the electromagnetic shielding filler is 15-25 parts by weight, and the resin component includes 60-85wt% of random polypropylene x, 5-20wt% of polyolefin elastomer y, and 5-20wt% of propylene impact copolymer z.

[0036] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the resin components of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:6, for example, it can be 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 and any value therebetween.

[0037] According to a preferred embodiment of the present invention, the ratio of Wb to Wy is 4:1-1:4.

[0038] According to the research conducted by the present inventors, when a double-layer or multi-layer film is co-extruded, when the ratio of Wb to Wy is within the range of the present invention, the impact performance of the film can be further improved, and at the same time the extrusion process will be more stable.

[0039] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min.

[0040] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min.

[0041] When the melt mass flow rates of the polypropylene composition A and the polypropylene composition B are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity and mechanical properties.

[0042] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A, the film layer B, or the resin component of the film layer B, or may have different compositions from the film layer A, the film layer B, or the resin component of the film layer B, or may be a mixture of two or three of the resin components of the polypropylene composition A, the film layer B, and the polypropylene composition B. When the polypropylene composite film has a structure of more than three layers, the film layer B is preferably used as the surface layer, such as a three-layer film including the film layer A, the film layer B, and the film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.

[0043] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.

[0044] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:2-1:1. Under this ratio, the composite film has good mechanical properties.

[0045] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.

[0046] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.

[0047] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.

[0048] According to the present invention, in order to improve other properties (such as stability, etc.) of the composite film, the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a lubricant, and an anti-adhesive agent (anti-adhesive agent). The specific type of the film-forming aid can be a conventional choice in the art, and will not be repeated here.

[0049] In the present invention, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight, relative to 100 parts by weight of the polypropylene composition.

[0050] According to some embodiments of the present invention, the polypropylene composition B further includes a coupling agent. The coupling agent can improve the compatibility between the resin component of the polypropylene composition and the electromagnetic shielding filler. The type, usage and dosage of the coupling agent can be conventionally selected in the art. For example, the coupling agent can be selected from titanate coupling agents, and the titanate coupling agent can be selected from one or more of monoalkoxy titanate, monoalkyl pyrophosphate titanate, coordination titanate and chelate titanate; preferably, the titanate coupling agent is selected from tetrabutyl titanate and / or tetraisopropyl titanate. Based on the total weight of the resin component as 100 parts by weight, the content of the coupling agent can be 1-6 parts by weight, preferably 4-6 parts by weight.

[0051] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0052] In the preparation method of the present invention, the process of mixing the polypropylene composition A and the optional antioxidant, lubricant and film-forming aid and extruding and granulating; and the process of mixing the polypropylene composition B and the optional antioxidant, lubricant, film-forming aid, electromagnetic shielding filler and coupling agent and extruding and granulating can generally include: mixing the polypropylene composition and the required additives in a high-speed mixer, adding the mixed materials to a twin-screw extruder for melt mixing and uniform extrusion and granulation, and drying to obtain pellets. Wherein, the processing temperature of the twin-screw extruder can be controlled to be 170-230°C.

[0053] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.

[0054] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.

[0055] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.

[0056] The polypropylene composite film of the present invention can be used in the field of packaging materials, and can be mainly used in the field of high-end packaging, such as fields requiring high impact resistance of the film, such as electronic product packaging.

[0057] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.

[0058] In the following examples and comparative examples:

[0059] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.

[0060] The properties of the polypropylene composition and the electromagnetic shielding film were tested according to the following method, and the film test results are shown in Table 1:

[0061] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.

[0062] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.

[0063] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.

[0064] (4) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.

[0065] (5) Shielding effectiveness: Tested in accordance with SJ20524 standard using flange coaxial test equipment, with the electromagnetic wave band ranging from 50 MHz to 1 GHz.

[0066] (6) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.

[0067] (7) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.

[0068] Example 1

[0069] This example is used to illustrate the preparation of the electromagnetic shielding polypropylene composite film provided by the present invention.

[0070] (1) Preparation of polypropylene composition A:

[0071] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is a polyolefin elastomer with the brand name 6102, an ethylene-propylene copolymer, with an ethylene structural unit content of 16 wt%, purchased from Exxon. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.5g / 10min.

[0072] (2) Preparation of polypropylene composition B:

[0073] Component x is a random polypropylene with a grade of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2g / 10min; component y is a polyolefin elastomer with a grade of 6102, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%, purchased from Exxon; component z is a propylene impact copolymer with a grade of EP200K, purchased from Zhongsha Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 13wt%, and a melt mass flow rate of 3.2g / 10min. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. Wb:Wy is 4:1. Based on the total weight of the above resin as 100 parts by weight, 25 parts by weight of Fe powder as an electromagnetic shielding filler and 5 parts by weight of tetrabutyl titanate as a coupling agent were added. The other steps were the same as step (1), and finally a polypropylene composition B pellet was obtained. The melt mass flow rate MFR of the resin component was tested. B =4.7g / 10min.

[0074] (3) Preparation of composite films:

[0075] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.

[0076] Example 2

[0077] This example is used to illustrate the preparation of the electromagnetic shielding polypropylene composite film provided by the present invention.

[0078] (1) Preparation of polypropylene composition A:

[0079] Component a is a propylene impact copolymer with the brand name M180R, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min, purchased from Shanghai Petrochemical; component b is a polyolefin elastomer with the brand name DF640, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%, purchased from Mitsui Co. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.1g / 10min.

[0080] (2) Preparation of polypropylene composition B:

[0081] Component x is random polypropylene with the brand name F500EPS, purchased from Shanghai Petrochemical; component y is a polyolefin elastomer with the brand name DF640, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%, purchased from Mitsui Company; component z is a propylene impact copolymer with the brand name M180R, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min, purchased from Shanghai Petrochemical. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. Wb:Wy is 1:4. Based on the sum of the mass of the above resins as 100 parts by weight, the electromagnetic shielding filler is conductive carbon black, and the addition amount is 15 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR of the resin component is tested. B =4.4g / 10min.

[0082] (3) Preparation of composite films:

[0083] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is also added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.

[0084] Example 3

[0085] This example is used to illustrate the preparation of the polypropylene composition and the composite film thereof provided by the present invention.

[0086] An electromagnetic shielding film was prepared according to Example 1, except that the electromagnetic shielding fillers were Fe powder and conductive carbon black, the Fe powder was 10 parts by weight, the conductive carbon black was 5 parts by weight, and the coupling agent tetrabutyl titanate was 3 parts by weight.

[0087] Example 4

[0088] This example is used to illustrate the preparation of the antistatic composite film provided by the present invention.

[0089] (1) Preparation of polypropylene composition A:

[0090] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =3.3g / 10min.

[0091] (2) Preparation of polypropylene composition B:

[0092] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 75 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 1:2. The other steps are the same as those in step (2), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR of its resin component is tested. B =5.5g / 10min.

[0093] (3) Preparation of composite films:

[0094] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.

[0095] Example 5

[0096] A polypropylene film was prepared according to the method of Example 2. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. Wb:Wy is 5:4. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.3g / 10min.

[0097] Example 6

[0098] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 99 parts by weight, and the mass fraction Wb of component b is 1 part by weight. Wb:Wy is 1:5. The pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.2g / 10min.

[0099] Example 7

[0100] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 25 parts by weight, and the mass fraction Wz of component z is 25 parts by weight. Wb:Wy is 4:5. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR of the resin components thereof was tested. B =4.0g / 10min.

[0101] Example 8

[0102] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 4:1. Finally, pellets of polypropylene composition B were obtained. The melt mass flow rate MFR of its resin components was tested. B =8.2g / 10min.

[0103] Example 9

[0104] A polypropylene film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition A, the mass fraction Wa of component a was 100 parts by weight, and component b was not added. Granules of the polypropylene composition A were obtained.

[0105] Comparative Example 1

[0106] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x.

[0107] Comparative Example 2

[0108] A composite film was prepared according to the method of Example 1, except that only the polypropylene composition B was used for extrusion casting into a single-layer film.

[0109] Comparative Example 3

[0110] A composite film was prepared according to the method of Example 1, except that the polypropylene composition B did not contain electromagnetic shielding filler.

[0111] Table 1

[0112]

[0113] From the results in Table 1, it can be concluded that the electromagnetic shielding polypropylene composite film provided by the present invention has good impact resistance, tensile properties and high heat sealing strength, so that the composite film after adding electromagnetic shielding filler can meet the use requirements of electromagnetic shielding while also achieving good mechanical properties, thereby broadening the application field of polypropylene film. The longitudinal (MD) tensile strength of the film of the present invention is ≥28MPa, preferably ≥35MPa. The pendulum impact strength is ≥0.4J, preferably ≥0.9J. And the heat sealing strength at 150°C is ≥12N / 15mm, preferably ≥14N / 15mm. The electromagnetic shielding effectiveness is ≥25dB, preferably ≥28dB.

[0114] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0115] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. An electromagnetic shielding polypropylene composite film, characterized in that: The polypropylene composite film is composed of at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and a polyolefin elastomer b, the polypropylene composition B comprises a resin component and an electromagnetic shielding filler, and the resin component comprises random polypropylene x, polyolefin elastomer y and propylene impact copolymer z; The polypropylene composition A comprises 70-95wt% of polypropylene a and 5-30wt% of polyolefin elastomer b; in the polypropylene composition B, based on 100 parts by weight of the resin component, the content of the electromagnetic shielding filler is 5-30 parts by weight, and the resin component comprises 50-90wt% of random polypropylene x, 5-30wt% of polyolefin elastomer y, and 2-30wt% of propylene impact copolymer z; Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the resin components of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:6; The propylene impact copolymer z is a propylene impact copolymer containing ethylene units; based on 100 parts by weight of the propylene impact copolymer z, the ethylene content of the propylene impact copolymer z is 1-12wt%; the polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an alpha olefin; When the polypropylene composite film has a structure of three or more layers, the film layer B is the surface layer.

2. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥28MPa; pendulum impact strength ≥0.4J; heat sealing strength at 150°C ≥12N / 15mm; and electromagnetic shielding effectiveness ≥25dB.

3. The electromagnetic shielding polypropylene composite film according to claim 2, characterized in that: The longitudinal tensile strength is ≥35MPa.

4. The electromagnetic shielding polypropylene composite film according to claim 2, characterized in that: The pendulum impact strength is ≥0.9J.

5. The electromagnetic shielding polypropylene composite film according to claim 2, characterized in that: The heat sealing strength at 150° C. is ≥14N / 15mm.

6. The electromagnetic shielding polypropylene composite film according to claim 2, characterized in that: The electromagnetic shielding effectiveness is ≥28dB.

7. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 3-10 g / 10 min.

8. The electromagnetic shielding polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 3-8 g / 10 min.

9. The electromagnetic shielding polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the resin component of the polypropylene composition B is 4-8 g / 10 min.

10. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.

11. The electromagnetic shielding polypropylene composite film according to claim 10, characterized in that: The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.

0.

12. The electromagnetic shielding polypropylene composite film according to claim 10, characterized in that: The propylene impact copolymer is a propylene impact copolymer containing ethylene units; based on 100 parts by weight of the propylene impact copolymer, the ethylene content of the propylene impact copolymer is 1-12wt%; the content of the copolymerized part containing ethylene units in the propylene impact copolymer is 3-15wt%; the melt mass flow rate of the propylene impact copolymer at 230°C and a load of 2.16kg is 1-10g / 10min.

13. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer z has a content of 3-15wt%; The propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

14. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The alpha olefin is C3-C 12 of alpha olefins.

15. The electromagnetic shielding polypropylene composite film according to claim 14, characterized in that: The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

16. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.

17. The electromagnetic shielding polypropylene composite film according to claim 16, characterized in that: The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.

18. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The electromagnetic shielding filler is a conductive metal filler and / or a carbon material.

19. The electromagnetic shielding polypropylene composite film according to claim 18, characterized in that: The conductive metal filler is conductive metal particles and / or conductive metal fibers.

20. The electromagnetic shielding polypropylene composite film according to claim 19, characterized in that: The metals in the conductive metal particles and the conductive metal fibers are each independently selected from one or more of silver, aluminum, copper, iron, nickel and stainless steel.

21. The electromagnetic shielding polypropylene composite film according to claim 18, characterized in that: The carbon material is one or more of carbon black, graphite, graphene and carbon nanotubes.

22. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: The polypropylene composition A comprises 80-95 wt % of polypropylene a and 5-20 wt % of polyolefin elastomer b.

23. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: In the polypropylene composition B, based on 100 parts by weight of the resin component, the content of the electromagnetic shielding filler is 15-25 parts by weight, and the resin component includes 60-85wt% of random polypropylene x, 5-20wt% of polyolefin elastomer y, and 5-20wt% of propylene impact copolymer z.

24. The electromagnetic shielding polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is Wb, based on the total weight of the resin components of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wb to Wy is 4:1-1:

4.

25. The electromagnetic shielding polypropylene composite film according to any one of claims 1 to 24, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:

1.

26. The electromagnetic shielding polypropylene composite film according to claim 25, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:2-1:

1.

27. The electromagnetic shielding polypropylene composite film according to any one of claims 1 to 24, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.

28. The electromagnetic shielding polypropylene composite film according to claim 27, characterized in that: The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.

29. The electromagnetic shielding polypropylene composite film according to claim 27, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.

30. The electromagnetic shielding polypropylene composite film according to claim 29, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.

31. The electromagnetic shielding polypropylene composite film according to claim 27, characterized in that: The lubricant is a PEG lubricant and / or a monoglyceride lubricant.

32. The electromagnetic shielding polypropylene composite film according to claim 27, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.

33. The electromagnetic shielding polypropylene composite film according to claim 32, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.

34. The electromagnetic shielding polypropylene composite film according to any one of claims 1 to 24, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.

35. The electromagnetic shielding polypropylene composite film according to claim 34, characterized in that: The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a lubricant and an anti-sticking agent.

36. The electromagnetic shielding polypropylene composite film according to claim 34, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.

37. The electromagnetic shielding polypropylene composite film according to claim 36, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.

38. The electromagnetic shielding polypropylene composite film according to any one of claims 1 to 24, characterized in that: The polypropylene composition B further comprises a coupling agent.

39. The electromagnetic shielding polypropylene composite film according to claim 38, characterized in that: The coupling agent is a titanate coupling agent.

40. The electromagnetic shielding polypropylene composite film according to claim 39, characterized in that: The titanate coupling agent is selected from one or more of monoalkoxy titanate, monoalkyl pyrophosphate titanate, coordination titanate and chelate titanate.

41. The electromagnetic shielding polypropylene composite film according to claim 40, characterized in that: The titanate coupling agent is selected from tetrabutyl titanate and / or tetraisopropyl titanate.

42. The electromagnetic shielding polypropylene composite film according to claim 38, characterized in that: Based on 100 parts by weight of the total weight of the resin component, the content of the coupling agent is 1-6 parts by weight.

43. The electromagnetic shielding polypropylene composite film according to claim 42, characterized in that: Based on 100 parts by weight of the total weight of the resin component, the content of the coupling agent is 4-6 parts by weight.

44. The method for preparing the electromagnetic shielding polypropylene composite film according to any one of claims 1 to 43, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.

45. The preparation method according to claim 44, characterized in that: The stretching is bidirectional stretching.

46. ​​Use of the electromagnetic shielding polypropylene composite film according to any one of claims 1 to 43 in the field of packaging materials.

47. The use according to claim 46, characterized in that The packaging is electronic product packaging.