A low-fog, high-impact heat-seal polypropylene composite film and its preparation method and application
By using a composite film composed of a specific composition in a polypropylene film, the problem that it is difficult for a polypropylene film to have both optical properties and impact resistance is solved, and a polypropylene composite film with high impact resistance, good optical and heat sealing properties is achieved.
Patent Information
- Application Number
- CN202111221954.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-20
AI Technical Summary
It is difficult for existing polypropylene films to have good optical properties and impact resistance at the same time, and the heat sealing performance is insufficient at low heat sealing temperatures.
A composite film composed of polypropylene composition A and polypropylene composition B is used, wherein polypropylene composition A includes polypropylene and polyolefin elastomer, and polypropylene composition B includes random polypropylene, polyolefin elastomer and propylene Impact copolymer, the average particle size of the rubber phase in the propylene impact copolymer is less than or equal to 1.8 μm, and the maximum particle size does not exceed 2.5 μm, and is prepared by extrusion casting method.
The film achieves high impact resistance, good optical properties and good heat sealing strength. The longitudinal tensile strength is ≥40MPa, the pendulum impact strength is ≥0.6J, the haze is ≤5%, and the heat sealing strength at 150℃ is ≥15N/15mm. .
Smart Images

Figure CN115991907B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of films, and in particular relates to a low-fog, high-impact, heat-seal polypropylene composite film and a preparation method and application thereof. Background Art
[0002] Polypropylene film can usually be made by methods such as casting and biaxial stretching, but polypropylene film made from homopolymer polypropylene raw materials usually has low impact strength. Polypropylene film is often used for packaging purposes, which requires the film to have high impact performance. At the same time, for the visualization and aesthetics of the contents, the film is also expected to have good optical properties. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomers can be added to polypropylene, but the films prepared by the above methods usually have high haze and poor optical properties such as transparency. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.
[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3, and the elastomer provides good impact resistance. However, this method has the problem of difficulty in uniform dispersion when the elastomer content is high, and it is still difficult to obtain a film with good optical properties. In addition, the amount of elastomer added will be limited, because when the amount added reaches a certain level, phase separation will occur, thereby limiting the further improvement of impact performance. Moreover, when the film is used for packaging purposes, it is usually hoped that it has good heat sealing performance at a lower heat sealing temperature. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good optical properties and impact resistance at the same time, and to provide a low-haze high-impact heat-seal polypropylene film and a preparation method thereof. The polypropylene film of the present invention has good impact resistance, optical properties and tensile properties at the same time, and has good heat-seal strength at a relatively low heat-seal temperature.
[0005] The first aspect of the present invention provides a low-haze high-impact polypropylene composite film, the polypropylene composite film comprising at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and a polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z; the propylene impact copolymer z comprises an elastic portion, the elastic portion forms a spherical or nearly spherical rubber phase, the average particle size of the rubber phase is less than or equal to 1.8 μm, and the maximum particle size does not exceed 2.5 μm.
[0006] The second aspect of the present invention provides a method for preparing the low-haze high-impact polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0007] The third aspect of the present invention provides the use of the low-haze and high-impact polypropylene composite film in the field of packaging materials.
[0008] The composite film prepared by the present invention has good impact resistance and optical properties, and the film has good heat sealing properties. The longitudinal (MD) tensile strength of the film is ≥40MPa, preferably ≥50MPa; the pendulum impact strength is ≥0.6J, preferably ≥1.8J; the film haze is ≤5%, preferably ≤2%; the heat sealing strength at 150°C is ≥15N / 15mm, preferably ≥19N / 15mm.
[0009] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Exemplary embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0011] Figure 1a and Figure 1b They are SEM photos of the cross-section of the impact-resistant polypropylene strips used in the embodiments of the present invention and the comparative examples, respectively.
[0012] Figure 2 This is an atomic force microscope photograph of a cross section of a thin film in one embodiment of the present invention. DETAILED DESCRIPTION
[0013] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0014] The present invention provides a low-haze high-impact polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and a polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z; the propylene impact copolymer z comprises an elastic part, which forms a spherical or nearly spherical rubber phase, wherein the average particle size of the rubber phase is less than or equal to 1.8 μm, and the maximum particle size does not exceed 2.5 μm, and preferably, the average particle size of the rubber phase is less than or equal to 1.5 μm, and the maximum particle size does not exceed 2 μm, which is determined by observing a cross section of a specimen under SEM.
[0015] In the present invention, the spherical and nearly spherical particles refer to particles whose aspect ratios are substantially in the range of 1 to 2. “Substantially” means that at least 90% of the rubber phase particles have aspect ratios in the range of 1 to 2.
[0016] The average particle size and maximum particle size of the rubber phase in the propylene impact copolymer in the raw material are determined by observing the cross section of the impact spline by the scanning electron microscope (SEM) method, and the impact spline is prepared according to the method specified in the standard GB / T8809-2015. For spherical particles, the diameter of the particle is measured; for nearly spherical particles, the longitudinal axis of the particle (the distance between the two points on the particle contour that are farthest apart) is measured. The average value of the above dimensions of 50 sample points is obtained by SEM photo observation as the average particle size, and the maximum value of the above dimensions in the above sample points is taken as the maximum particle size.
[0017] According to the research of the inventors, when the average particle size of the rubber phase in the propylene impact copolymer is within the above range, the impact resistance of the film can be improved, and the size of the rubber phase in the film can be reduced, thereby improving the optical performance. In addition, polyolefin elastomers are usually dispersed in the polypropylene composition with this particle size range. Therefore, controlling the size range of the rubber phase in the propylene impact copolymer can also solve the problem of the decline of impact resistance and optical performance caused by the large size difference of the rubber phases of different components. At the same time, it is found that by controlling the rubber phase particle size of the propylene impact copolymer, the components in the heat seal layer can better play a synergistic effect, and while reducing the heat seal temperature, the heat seal strength can also be effectively improved.
[0018] In the present invention, the meaning of the term "average particle size of the rubber phase" is well known to those skilled in the art. The particle size of the rubber phase is measured and statistically obtained by scanning and observing the impact spline section after gold spraying using a scanning electron microscope EM-30AX of COXEM of South Korea.
[0019] According to some embodiments of the present invention, there is a dispersed strip-shaped rubber phase in the composite film, the rubber phases are arranged parallel to each other, and the average width of the rubber phase is 20-200nm, and the average aspect ratio is 5-15. The "dispersed" mentioned herein means that the rubber phase is not continuously distributed in the composite film. The rubber phase can be seen by observing the cross section of the composite film cut along the transverse direction (TD) through an atomic force microscope (AFM), such as Figure 2 As shown in the black part, the rubber phase is in the form of multiple strips uniformly dispersed in the film matrix.
[0020] Herein, the "strip shape" refers to a shape whose aspect ratio is generally greater than 2.
[0021] The meaning of aspect ratio is well known to those skilled in the art. For strip particle testing, aspect ratio has the same concept as length-to-width ratio, that is, the ratio of the longest diameter passing through the inside of the particle to the longest diameter perpendicular to it. The former also corresponds to the length of the particle, and the latter corresponds to the width of the particle.
[0022] The average width and average aspect ratio are measured by observing the cross section of the composite film cut along the transverse direction (TD) using an atomic force microscope. Based on 200 sample points, the average value of the horizontal axis dimension of the rubber phase is calculated as the average width, and the average value of the aspect ratio of the rubber phase is calculated as the average aspect ratio.
[0023] The machine direction (MD) refers to the machining direction. The transverse direction (TD) refers to the direction perpendicular to the machining direction.
[0024] In the composite film of the invention, the rubber phases are advantageously arranged parallel to each other.
[0025] Herein, the term "parallel arrangement" means that the transverse cross sections of the rubber phase are arranged parallel to each other along a certain direction. This excludes a small amount of rubber phase particles arranged in different directions in a local area due to the preparation process and inconsistent with the overall arrangement direction of the rubber phase particles in the entire composite film, as well as rubber phase particles that cannot be clearly observed due to the preparation process or AFM method.
[0026] Herein, "parallel arrangement" includes substantially parallel conditions. The angle between the transverse cross sections of the rubber phases is not greater than about 10 degrees, preferably less than about 5 degrees.
[0027] By controlling the size of the rubber phase in the propylene impact copolymer, the size of the rubber phase in the composite film can be made within the above range.
[0028] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥40MPa, preferably longitudinal tensile strength ≥50MPa; pendulum impact strength ≥0.6J, preferably pendulum impact strength ≥1.8J; film haze ≤5%, preferably haze ≤2%; heat sealing strength at 150°C ≥15N / 15mm, preferably heat sealing strength at 150°C ≥19N / 15mm.
[0029] According to some embodiments of the present invention, the polypropylene a can be selected from homopolypropylene and / or propylene impact copolymer. Preferably, the homopolypropylene has a melt mass flow rate of 2-15g / 10min at 230°C and a load of 2.16kg, an isotacticity of greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available. For example, homopolypropylene with a grade of PPH-FA03 of Qingdao Refining and Chemical and homopolypropylene with a grade of FC801 of Shanghai Petrochemical. Alternatively, it can be prepared by conventional methods in the art.
[0030] According to the present invention, the propylene impact copolymer z is preferably a propylene impact copolymer containing ethylene units, the copolymerization part containing ethylene units forms the elastic part, and the copolymerization part containing ethylene units is preferably selected from ethylene-propylene copolymerization part and ethylene-butene copolymerization part. The elastic part can be shown as a spherical or nearly spherical rubber phase in the scanning electron microscope photo of the impact sample strip of the propylene impact copolymer.
[0031] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.
[0032] Based on the total weight of the propylene impact copolymer z, the content of the copolymerized part containing ethylene units in the propylene impact copolymer is preferably 3-15wt%, more preferably 7-12wt%. 13 C NMR determination.
[0033] The ethylene content of the propylene impact copolymer z is preferably 1-12 wt % based on the total weight of the propylene impact copolymer z. In the room temperature xylene solubles of the propylene impact copolymer z, the ethylene unit content is preferably not more than 40 wt %. The ethylene unit group [EEE] content is preferably not more than 20 wt %. 13 C NMR determination.
[0034] Preferably, the propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.
[0035] The propylene impact copolymer may have a block structure or include a propylene block copolymer.
[0036] Propylene impact copolymers meeting the above characteristics are commercially available, such as Shanghai Petrochemical's F200R propylene impact copolymer, Korea Hyosung's J410F propylene impact copolymer, and Maoming Petrochemical's PPB-M02D propylene impact copolymer.
[0037] The propylene impact copolymer can also be prepared by a continuous polymerization process in the presence of a Ziegler-Natta catalyst with high stereoselectivity. The continuous polymerization process means that the preparation process includes at least two sequential steps, wherein the elastic part and the non-elastic part are each prepared in a separate step, and, except for the first step, the latter step is carried out in the presence of the polymer formed in the previous step and the catalyst used in the previous step.
[0038] The polypropylene a may be selected from propylene impact copolymers which are the same as or different from the propylene impact copolymer z, preferably satisfying the above conditions.
[0039] According to some embodiments of the present invention, the polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an alpha olefin. The alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
[0040] The polyolefin elastomers meeting the above characteristics are commercially available, for example, polyolefin elastomers with the trade name of 8200 from Dow, polyolefin elastomers with the trade name of 8411 from Dow, polyolefin elastomers with the trade name of DF840 from Mitsui, and polyolefin elastomers with the trade name of VM3980 from Exxon, or can be prepared by conventional methods in the art.
[0041] When polyolefin elastomer is used in the composite film, the elastic part of the propylene impact copolymer and the polyolefin elastomer form a dispersed rubber phase in the composite film, which is in the form of strips and arranged parallel to each other. The specific features are as described above and will not be repeated here.
[0042] The presence of the polyolefin elastomer can advantageously compensate for the possible uneven distribution of the rubber phase in the propylene impact copolymer, thereby improving the uniformity of the impact properties of the film at various locations.
[0043] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.
[0044] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.
[0045] Random polypropylenes meeting the above characteristics are commercially available, such as Yanshan Petrochemical's F5006 random polypropylene, Shanghai Petrochemical's F500EPS random polypropylene, and Shanghai Petrochemical's F800EPS random polypropylene. Alternatively, they can be prepared by conventional methods in the art.
[0046] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-95 wt % of the polypropylene a and 5-50 wt % of the polyolefin elastomer b.
[0047] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 80-95 wt% of polypropylene a and 5-20 wt% of polyolefin elastomer b.
[0048] The elastomer or impact copolymer in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular segments of the homopolymer phase of the homopolymer polypropylene and the impact copolymer are relatively regular, crystallization and orientation occur during the film preparation process, providing good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the rubber phase can be evenly distributed in the film, and the shape and size of the rubber phase can meet the requirements of the refractive index, so a film with good optical properties can be obtained, so that the film has good impact performance and optical properties at the same time; at the same time, under this ratio, the composition also contains enough homopolymer phase, so that the film has good mechanical properties.
[0049] According to some embodiments of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-90 wt% of the polypropylene x, 5-40 wt% of the polyolefin elastomer y and 2-30 wt% of the propylene impact copolymer z.
[0050] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 60-85 wt% of polypropylene x, 5-20 wt% of polyolefin elastomer y and 5-20 wt% of propylene impact copolymer z.
[0051] According to the research of the present inventors, when the polypropylene composition B adopts this ratio and the surface layer in the composite film is made of the polypropylene composition B, the added propylene impact copolymer can give the film good mechanical properties and can further improve the heat sealing performance of the film. At the same time, when the rubber phase in the propylene impact copolymer is within the scope of the present invention, it will not affect the overall optical properties of the composite film.
[0052] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min.
[0053] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min, preferably 4-9 g / 10 min.
[0054] When the melt mass flow rates of the polypropylene composition A and the polypropylene composition B are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity, mechanical properties and optical properties.
[0055] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A or the film layer B, or may have different compositions from the film layer A or the film layer B, or may be a mixture of a polypropylene composition A and a polypropylene composition B. When the polypropylene composite film has a structure of three or more layers, the film layer B is preferably used as a surface layer, such as a three-layer film including a film layer A, a film layer B, and a film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.
[0056] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.
[0057] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:2-1:1. Under this ratio, the composite film has good mechanical properties.
[0058] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.
[0059] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.
[0060] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.
[0061] According to the present invention, in order to improve other properties of the composite film (such as stability, antistatic property, etc.), the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-adhesive agent (anti-adhesive agent) and an antistatic agent. The specific type of the film-forming aid can be a conventional choice in the art, and the present invention is not particularly limited thereto.
[0062] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.
[0063] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0064] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.
[0065] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.
[0066] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.
[0067] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.
[0068] By using the preparation method according to the present invention, the rubber phase contained in the propylene impact copolymer as the raw material is deformed during the preparation process of the composite film, changing from a spherical or nearly spherical shape to a strip shape, and is oriented in a certain direction, i.e. arranged in parallel, and such a microstructure is maintained in the final composite film product, thereby obtaining a composite film according to the present invention with good impact resistance and optical properties.
[0069] Advantageously, the polyolefin elastomer used also deforms during the preparation of the composite film, becoming a strip-shaped rubber phase and oriented in a certain direction, i.e. arranged in parallel, and such a microstructure is maintained in the final composite film product, while interacting synergistically with the rubber phase from the propylene impact copolymer, thereby further improving the impact resistance, optical properties and other properties of the composite film.
[0070] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as in the field of high-end packaging that requires both high impact resistance and optical properties of the film, including but not limited to battery packaging, electronic product packaging or food (especially high-end food) packaging.
[0071] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0072] In the following examples and comparative examples:
[0073] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.
[0074] The polypropylene composition and film properties were tested according to the following method, and the film test results are shown in Table 1:
[0075] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.
[0076] (2) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.
[0077] (3) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.
[0078] (4) Film haze: measured according to the method specified in GB / T 2410-2008.
[0079] (5) Film thickness: The film thickness was tested using a thickness gauge model 7301 produced by Mitutoyo of Japan.
[0080] (6) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.
[0081] (7) Atomic force microscopy (AFM) images: A Dimension FastScan Icon atomic force microscope (AFM) from Bruker Corporation of the United States was used to scan and observe the cross-section of the thin film sample along the transverse cut using the quantitative nanomechanical scanning mode.
[0082] (8) Average particle size and maximum particle size of the rubber phase of the propylene impact copolymer in the raw material: The EM-30AX scanning electron microscope of COXEM, Korea, was used to scan and observe the impact spline section after gold spraying, and the particle size of the rubber phase was measured and counted to obtain the average particle size and maximum particle size. For spherical particles, the diameter of the particle was measured; for nearly spherical particles, the longitudinal axis of the particle (the distance between the two points on the contour of the object that are farthest apart) was measured. Based on 50 sample points, the maximum value of the above size was obtained as the maximum particle size, and the average value of the above size was calculated as the average particle size.
[0083] (9) Method for determining the average width and average aspect ratio of the rubber phase of the film: Using the Dimension FastScan Icon atomic force microscope of Bruker Corporation of the United States, the quantitative nanomechanical scanning mode was used to scan and observe the cross section of the film sample, and the width of the rubber phase was measured and counted to obtain the average width (based on 200 sample points). The aspect ratio of the rubber phase is the ratio of its length direction to its width direction. After measurement, calculation and statistics, the average aspect ratio (based on 200 sample points) was obtained.
[0084] (10) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.
[0085] (11) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.
[0086] (12) The copolymer content containing ethylene units, ethylene unit content, and ethylene unit group [EEE] content in the propylene impact copolymer: 13 C NMR determination.
[0087] 13 C NMR was measured using a 400MHz nuclear magnetic resonance spectrometer (NMR) from Bruker, Switzerland, model AVANCE III. The solvent was deuterated o-dichlorobenzene, 250mg sample / 2.5ml solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2mg of BHT antioxidant was added to the sample. The sample was dissolved at 140℃ and collected. 13 C-NMR, test temperature 125°C, probe head specification 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan times 6000 times.
[0088] Example 1
[0089] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0090] (1) Preparation of polypropylene composition A:
[0091] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is polyolefin elastomer with the brand name 8411, purchased from Dow, and is an ethylene-1-octene copolymer with an octene structural unit content of 36 wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.4g / 10min.
[0092] (2) Preparation of polypropylene composition B:
[0093] Component x is a random polypropylene with a brand name of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer with a brand name of 8200, purchased from Dow, which is an ethylene-1-octene copolymer with an octene structural unit content of 38 wt%; component z is a propylene impact copolymer with a brand name of PPB-M02D, with an average rubber phase size of 1.4 μm and a maximum rubber phase size of 1.9 μm, purchased from Maoming Petrochemical, with an ethylene content of 8 wt%, an ethylene-propylene copolymer content of 10 wt%, and an ethylene unit content of 36.3 wt% and an ethylene unit group [EEE] content of 18.5 wt% in its room temperature xylene solubles, and a melt mass flow rate of 1.5 g / 10 min. The components prepared above were weighed and mixed according to the proportion, wherein the mass fraction Wx of component x was 85 parts by weight, the mass fraction Wy of component y was 5 parts by weight, and the mass fraction Wz of component z was 10 parts by weight. The other steps were the same as step (1), and finally a polypropylene composition B pellet was obtained. The melt mass flow rate MFR B =4.8g / 10min.
[0094] (3) Preparation of composite films:
[0095] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.
[0096] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 128 nm, and the average aspect ratio was 5.2.
[0097] Example 2
[0098] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0099] (1) Preparation of polypropylene composition A:
[0100] Component a is a propylene impact copolymer with a grade of F200R, purchased from Shanghai Petrochemical, with an average rubber phase size of 800nm, a maximum rubber phase size of 1μm, an ethylene content of 9.1wt%, an ethylene-propylene copolymer content of 12.2wt%, an ethylene unit content of 38.1wt% in xylene solubles at room temperature, an ethylene unit group [EEE] content of 13.6wt%, and a melt mass flow rate of 2.1g / 10min. Figure 1a The SEM photo of the cross section of component a is shown in Figure 1. Component b is a polyolefin elastomer with a grade of DF840, purchased from Mitsui Co., Ltd., which is an ethylene-1-butene copolymer with a butene structural unit content of 25wt%. The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.6g / 10min.
[0101] (2) Preparation of polypropylene composition B:
[0102] Component x is a random polypropylene with the brand name F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3g / 10min; component y is a polyolefin elastomer with the brand name DF840, purchased from Mitsui & Co., Ltd., with a butene structural unit content of 25wt%; component z is a propylene impact copolymer with the brand name F200R. The above-prepared components are weighed and mixed according to the proportions, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =4.3g / 10min.
[0103] (3) Preparation of composite films:
[0104] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the film casting process, the temperature of the casting chill roll is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.
[0105] The atomic force microscope photo of the cross section of the composite film is as follows Figure 2 As shown. The black part is the rubber phase, which is dispersed, strip-shaped, and arranged parallel to each other. The average width of the rubber phase is 88nm, and the average aspect ratio is 7.5.
[0106] Example 3
[0107] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0108] (1) Preparation of polypropylene composition A:
[0109] Component a is homopolypropylene with the brand name FC801, purchased from Shanghai Petrochemical, with a melt mass flow rate of 7.8 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.8; component b is polyolefin elastomer with the brand name VM3980, purchased from Exxon, and is a propylene-ethylene copolymer with an ethylene structural unit content of 9 wt%. The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 85 parts by weight, and the mass fraction Wb of component b is 15 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =7.4g / 10min.
[0110] (2) Preparation of polypropylene composition B:
[0111] Component x is a random polypropylene with a brand name of F800EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 8.2 g / 10 min; component y is a polyolefin elastomer with a brand name of VM3980, purchased from Exxon, which is a propylene-ethylene copolymer with an ethylene structural unit content of 9 wt%; component z is a propylene impact copolymer with a brand name of J410F, purchased from Hyosung of South Korea, with an average rubber phase size of 600 nm, a maximum rubber phase size of 800 nm, an ethylene content of 5.3 wt%, an ethylene-propylene copolymer content of 7.2 wt%, and an ethylene unit content of 26.0 wt% and an ethylene unit group [EEE] content of 6.9 wt% in its room temperature xylene solubles, and a melt mass flow rate of 4.6 g / 10 min. The components prepared above were weighed and mixed according to the proportion, wherein the mass fraction Wx of component x was 85 parts by weight, the mass fraction Wy of component y was 10 parts by weight, and the mass fraction Wz of component z was 5 parts by weight. The other steps were the same as step (1), and finally a pellet of polypropylene composition B was obtained. The melt mass flow rate MFR B =8.4g / 10min.
[0112] (3) Preparation of composite films:
[0113] The preparation process is the same as step (3) of Example 1.
[0114] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 54 nm, and the average aspect ratio was 9.8.
[0115] Example 4
[0116] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0117] (1) Preparation of polypropylene composition A:
[0118] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =3.5g / 10min.
[0119] (2) Preparation of polypropylene composition B:
[0120] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR B =5.5g / 10min.
[0121] (3) Preparation of composite films:
[0122] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0123] Example 5
[0124] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0125] (1) Preparation of polypropylene composition A:
[0126] The steps are the same as those in Example 2, except that the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =4.0g / 10min.
[0127] (2) Preparation of polypropylene composition B:
[0128] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 13 parts by weight, and the mass fraction Wz of component z is 2 parts by weight. Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate MFR thereof is tested. B =8.2g / 10min.
[0129] (3) Preparation of composite films:
[0130] The steps are the same as those in Example 2. The film thickness is 50 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 2:1.
[0131] Example 6
[0132] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0133] (1) Preparation of polypropylene composition A:
[0134] The steps are the same as in Example 3.
[0135] (2) Preparation of polypropylene composition B:
[0136] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 30 parts by weight, and component y is a polyolefin elastomer with a grade of 8411, which is an ethylene-1-octene copolymer with an octene structural unit content of 36wt%, purchased from Dow. The mass fraction Wz of component z is 20 parts by weight. Finally, a pellet of polypropylene composition B is obtained, and its melt mass flow rate MFR is tested. B =8.6g / 10min.
[0137] (3) Preparation of composite films:
[0138] The steps are the same as those in Example 3. The film thickness is 50 μm, wherein the ratio of the thickness of the upper surface layer to the thickness of the core layer is 1:4.
[0139] When the composite film is observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases can be seen. The average width of the rubber phase is 28 nm, and the average aspect ratio is 14.5.
[0140] Example 7
[0141] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0142] (1) Preparation of polypropylene composition A:
[0143] The steps are the same as in Example 1.
[0144] (2) Preparation of polypropylene composition B:
[0145] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 30 parts by weight. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR B =4.3g / 10min.
[0146] (3) Preparation of composite films:
[0147] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0148] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 147 nm, and the average aspect ratio was 6.3.
[0149] Example 8
[0150] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 50 parts by weight, and the mass fraction Wb of component b is 50 parts by weight. Finally, the polypropylene composition A pellets were obtained, and the melt mass flow rate MFR A =3.6g / 10min.
[0151] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 120 nm, and the average aspect ratio was 5.5.
[0152] Example 9
[0153] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 40 parts by weight, the mass fraction Wy of component y is 30 parts by weight, and the mass fraction Wz of component z is 30 parts by weight. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR B =4.2g / 10min.
[0154] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 145 nm, and the average aspect ratio was 7.4.
[0155] Example 10
[0156] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 40 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR B =5.3g / 10min.
[0157] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 102 nm, and the average aspect ratio was 9.3.
[0158] Comparative Example 1
[0159] A polypropylene film was prepared according to the method of Example 1. The difference was that in the preparation process of the polypropylene composition B, the propylene impact copolymer z was replaced with a propylene impact copolymer with a grade of F780R, purchased from Shanghai Petrochemical, with an average rubber phase size of 2.0 μm, a maximum rubber phase size of 3.0 μm, an ethylene content of 9.0 wt%, an ethylene-propylene copolymer content of 17.1 wt%, a melt mass flow rate of 7.3 g / 10 min, Figure 1b The SEM photo of the cross section of the propylene impact copolymer strip is shown in Figure 1. Finally, the polypropylene composition B pellets were obtained. The melt mass flow rate MFR B =7.9 g / 10 min. Film thickness is 50 μm.
[0160] Comparative Example 2
[0161] A polypropylene film was prepared according to the method of Example 2. The difference was that component a in composition A and component z in composition B were replaced with a propylene impact copolymer with a grade of F780R to obtain a pellet of polypropylene composition A. The melt mass flow rate MFR A =7.3 g / 10 min. The obtained polypropylene composition B pellets were tested for their melt mass flow rate MFR B =6.5g / 10min. Film thickness is 50μm.
[0162] Comparative Example 3
[0163] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x.
[0164] Comparative Example 4
[0165] A composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x and component y, wherein the mass fraction Wx of component x was 85 parts by weight, and the mass fraction Wy of component y was 15 parts by weight.
[0166] Comparative Example 5
[0167] A composite film was prepared according to the method of Example 2. The difference was that the polypropylene composition B contained only component x and component z, wherein the mass fraction Wx of component x was 70 parts by weight, and the mass fraction Wz of component z was 30 parts by weight.
[0168] Table 1
[0169]
[0170] From the results of the embodiments in Table 1, it can be concluded that the composite film prepared by using the polypropylene composition provided by the present invention has good impact resistance, optical properties and tensile properties, and has good heat sealing strength. The longitudinal tensile strength of the film of the present invention is ≥40MPa, the film haze is ≤5%, the pendulum impact strength is ≥0.6J, and the heat sealing strength at 150°C is ≥15N / 15mm. It can be seen from the preferred embodiments that the longitudinal tensile strength of the film of the present invention is ≥50MPa, the film haze is ≤2%, the pendulum impact strength is ≥1.8J, and the heat sealing strength at 150°C is ≥19N / 15mm. It can be seen from the comparative example that the composite film prepared by using the polypropylene composition prepared by the impact-resistant polypropylene copolymer with a rubber phase size outside the present invention has poor optical properties and impact resistance. Moreover, during extrusion casting, the film surface is unstable, and it is difficult to obtain a film with uniform thickness.
[0171] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0172] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A low haze, high impact heat-seal polypropylene composite film, It is characterized in that The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises polypropylene a and a polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y and a propylene impact copolymer z; the propylene impact copolymer z comprises an elastic part, the elastic part forms a spherical or nearly spherical rubber phase, the average particle size of the rubber phase is less than or equal to 1.8 μm, and the maximum particle size does not exceed 2.5 μm; Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-95wt% of polypropylene a and 5-50wt% of polyolefin elastomer b; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-90wt% of polypropylene x, 5-40wt% of polyolefin elastomer y and 2-30wt% of propylene impact copolymer z; Film layer B is the surface layer in the composite film; The propylene impact copolymer is a propylene impact copolymer containing ethylene units, and the copolymerized part containing ethylene units forms the elastic part; the ethylene content of the propylene impact copolymer is 1-12wt%; the content of the copolymerized part containing ethylene units in the propylene impact copolymer is 3-15wt%; in the room temperature xylene soluble matter of the propylene impact copolymer, the ethylene unit content does not exceed 40wt%, the ethylene unit group EEE content does not exceed 20wt%, and the elastic part is formed by the propylene impact copolymer. 13 C NMR determination; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; at 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min.
2. The low haze high impact heat seal polypropylene composite film according to claim 1, It is characterized in that The average particle size of the rubber phase is less than or equal to 1.5 μm, and the maximum particle size does not exceed 2 μm.
3. The low haze high impact heat seal polypropylene composite film according to claim 1, It is characterized in that There are dispersed strip-shaped rubber phases in the polypropylene composite film. The rubber phases are arranged parallel to each other, and the average width of the rubber phases is 20-200nm and the average aspect ratio is 5-15.
4. The low haze high impact heat seal polypropylene composite film according to claim 3, It is characterized in that The angles between the transverse sections of the rubber phase are no greater than 10 degrees, which is determined by observing the cross section of the composite film cut along the transverse direction (TD) using an atomic force microscope.
5. The low haze high impact heat seal polypropylene composite film according to claim 4, It is characterized in that The angles between the transverse sections of the rubber phase are less than 5 degrees, which is determined by observing the cross section of the composite film cut along the transverse direction (TD) using an atomic force microscope.
6. The low haze, high impact heat seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥40MPa; pendulum impact strength ≥0.6J; film haze ≤5%; heat sealing strength at 150°C ≥15N / 15mm.
7. The low haze high impact heat seal polypropylene composite film according to claim 6, It is characterized in that The longitudinal tensile strength of the polypropylene composite film is ≥50MPa.
8. The low haze high impact heat seal polypropylene composite film according to claim 6, It is characterized in that The pendulum impact strength of the polypropylene composite film is ≥1.8J.
9. The low haze high impact heat seal polypropylene composite film according to claim 6, It is characterized in that The haze of the polypropylene composite film is ≤2%.
10. The low haze, high impact heat-seal polypropylene composite film according to claim 6, It is characterized in that The heat sealing strength of the polypropylene composite film at 150° C. is ≥19N / 15mm.
11. The low haze high impact heat seal polypropylene composite film according to claim 1, It is characterized in that At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 3-8 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 4-9 g / 10 min.
12. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The polypropylene a is selected from homopolypropylene and / or propylene impact copolymer.
13. The low haze high impact heat seal polypropylene composite film according to claim 12, It is characterized in that The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.
0.
14. The low haze high impact heat seal polypropylene composite film according to claim 1, It is characterized in that The propylene impact copolymer meets the following conditions: the propylene impact copolymer contains an elastic portion, which forms a spherical or nearly spherical rubber phase, the average particle size of the rubber phase is less than or equal to 1.5 μm, and the maximum particle size does not exceed 2 μm; and / or the melt mass flow rate of the propylene impact copolymer at 230° C. and a load of 2.16 kg is 1-10 g / 10 min.
15. The low haze high impact heat seal polypropylene composite film according to claim 14, It is characterized in that The copolymerization part containing ethylene units in the propylene impact copolymer has a content of 7-12 wt %.
16. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The propylene impact copolymer z is a propylene impact copolymer containing ethylene units, and the copolymerized part containing ethylene units forms the elastic part; The propylene impact copolymer z has an ethylene content of 1-12 wt % based on the total weight of the propylene impact copolymer z; and / or, The copolymerization part containing ethylene units in the propylene impact copolymer z has a content of 3-15 wt%; and / or, In the room temperature xylene solubles of the propylene impact copolymer z, the ethylene unit content is not more than 40wt%, and / or the ethylene unit group EEE content is not more than 20wt%. 13 C NMR measurement; and / or, The propylene impact copolymer z has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.
17. The low haze high impact heat seal polypropylene composite film according to claim 16, It is characterized in that The content of the copolymerized part containing ethylene units in the propylene impact copolymer z is 7-12 wt %.
18. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an α-olefin.
19. The low haze high impact heat seal polypropylene composite film according to claim 18, It is characterized in that The alpha olefin is C 3 -C 12 of alpha olefins.
20. The low haze high impact heat seal polypropylene composite film according to claim 19, It is characterized in that The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
21. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The random polypropylene x is a copolymer of propylene and ethylene and / or butene; and / or, The random polypropylene x has a melt mass flow rate of 2-10 g / 10 min at 230° C. and a load of 2.16 kg.
22. The low haze high impact heat seal polypropylene composite film according to claim 21, It is characterized in that The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.
23. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 80-95 wt% of the polypropylene a and 5-20 wt% of the polyolefin elastomer b.
24. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 60-85 wt% of the polypropylene x, 5-20 wt% of the polyolefin elastomer y and 5-20 wt% of the propylene impact copolymer z.
25. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:
1.
26. The low haze high impact heat seal polypropylene composite film according to claim 25, It is characterized in that In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:2-1:
1.
27. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that When the polypropylene composite film has a structure of three or more layers, the film layer A is the middle layer.
28. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.
29. The low haze high impact heat seal polypropylene composite film according to claim 28, It is characterized in that The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.
30. The low haze, high impact heat-seal polypropylene composite film according to claim 28, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.
31. The low haze, high impact heat-seal polypropylene composite film according to claim 30, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.
32. The low haze, high impact heat seal polypropylene composite film according to claim 28, It is characterized in that The lubricant is a PEG lubricant and / or a monoglyceride lubricant.
33. The low haze, high impact heat seal polypropylene composite film according to claim 28, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.
34. The low haze, high impact heat-seal polypropylene composite film according to claim 33, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.
35. The low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 5, It is characterized in that The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.
36. The low haze, high impact heat seal polypropylene composite film according to claim 35, It is characterized in that The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-sticking agent and an antistatic agent.
37. The low haze, high impact heat seal polypropylene composite film according to claim 35, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.
38. The low haze, high impact heat-seal polypropylene composite film according to claim 37, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.
39. The method for preparing the low haze high impact heat seal polypropylene composite film according to any one of claims 1 to 38, include: The raw material composition for forming each layer is extruded and cast after an optional granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.
40. The preparation method according to claim 39, It is characterized in that The stretching is bidirectional stretching.
41. Use of the low haze, high impact, heat-seal polypropylene composite film according to any one of claims 1 to 38 in the field of packaging materials.
42. The use according to claim 41, It is characterized in that The packaging is battery packaging, electronic product packaging or food packaging.
Citation Information
Patent Citations
Toughening type three-layer coextru-laminated film and preparation method thereof
CN101913279A
Polypropylene combination and stretched thin film prepared from same
CN102050991A
Polypropylene composition and polypropylene pellet
CN104327369A
Polymer membrane, and preparation method thereof
CN105623079A
Heat sealing layer, CPP film, preparation method thereof and aluminum-plastic film
CN108943932A