Aromatic oxime adsorption material and preparation method and application thereof

By acylating aromatic cyanide diamines and aromatic cyanide dibasic acid anhydrides under an inert atmosphere and cross-linking them with aldehyde compounds, an adsorption material with specific ion channels is formed, which solves the problem of poor selectivity and environmental resistance of existing uranium adsorption materials. It solves the problem of insufficient adsorption capacity and achieves efficient and stable uranium adsorption effect.

CN115999516BActive Publication Date: 2024-10-15EAST CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211354706.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-01
Publication Date
2024-10-15
Estimated Expiration
2042-11-01

AI Technical Summary

Technical Problem

Existing uranium adsorption materials have problems such as poor selectivity, low adsorption efficiency and poor environmental tolerance. It is difficult to effectively capture uranium from seawater. At the same time, they have a high adsorption capacity for other competitive ions, and their single structure results in adsorption capacity and efficiency. Low.

Method used

By acylating aromatic cyanide diamines and aromatic cyanide dibasic acid anhydrides under an inert atmosphere, amine-terminated oligomers are obtained and cross-linked with aldehyde compounds to form adsorption materials with specific ion channels. Improve selectivity and surface hydrophilicity while introducing aromatic rings to enhance environmental tolerance.

Benefits of technology

It has achieved high selectivity and high adsorption capacity for uranium in seawater. After 10 adsorption and desorption cycles, the adsorption capacity retention rate is greater than 98%, which significantly improves the selectivity and environmental tolerance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115999516B_ABST
    Figure CN115999516B_ABST
Patent Text Reader

Abstract

The present invention provides an aromatic oxime adsorption material and a preparation method and application thereof, belonging to the field of uranium adsorption materials. The present invention performs an acylation reaction on aromatic diamine cyanide and aromatic dibasic cyanide anhydride to obtain an amino-terminated oligomer with adjustable molecular scale, and then adds an aldehyde compound for cross-linking reaction to obtain a uranium adsorption material with a specific "ion channel"; wherein the appropriate ion channel radius greatly improves the selectivity of the adsorption material; by selecting aromatic diamine cyanide and aromatic dibasic cyanide anhydride as reaction monomers, the surface hydrophilicity of the adsorption material is enhanced, the diffusion rate of uranyl at the phase interface is improved, and an aromatic ring is introduced at the same time, the electronic conjugated structure of the aromatic ring effectively reduces the positive charge of the oxime carbon cation, hinders the attack of the oxime by the nucleophilic reagent, and improves the environmental tolerance of the adsorption material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of uranium adsorption materials, and in particular relates to an aromatic oxime adsorption material and a preparation method and application thereof. Background Art

[0002] As a clean energy, nuclear energy has become one of the largest contributors to zero carbon emissions. The demand for clean energy using uranium as raw material will continue to rise. The ocean has 4.5 billion tons of uranium resources, which is an ideal "uranium mine" for obtaining uranium resources. Among the many methods for enriching and separating uranium resources, the adsorption method has become the most effective and commonly used method for obtaining uranium resources from seawater due to its advantages such as simple operation, low environmental pollution and high economic benefits.

[0003] Vukovic of Oak Ridge National Laboratory in Tennessee, USA, pointed out through theoretical calculations and related characterization that unpaired electrons in elements such as nitrogen, oxygen, and phosphorus can occupy empty orbitals of uranium, so related sites (such as NO) can form stable combinations with uranium. In the prior art, suitable monomers are usually selected and polymer materials with specific pore structures are prepared through specific reactions. However, the adsorbent materials obtained by the preparation methods provided by the prior art still have the following problems: (1) Poor selectivity. While capturing uranium, the current uranium adsorbent materials also produce considerable adsorption of other competitive ions such as vanadium, iron, copper and other elements. For example, the more common oxime derivatives have better adsorption performance for vanadium than for uranium. (2) Weak surface hydrophilicity and low adsorption efficiency. The good hydrophilicity of the adsorbent surface is beneficial to the rapid diffusion of uranyl ions on the surface, thereby increasing the collision probability of active sites with uranium. Vice versa. (3) The adsorption structure is single and the environmental tolerance is poor. The adsorption structure is simple, mainly manifested in the small number of surface active sites and types, resulting in low adsorption capacity and efficiency: For the widely studied polyamidoximes, the carbon cations in cycloimide dioxime are easily affected by nucleophiles (such as H 2 O) and hydrolyzes, resulting in the inactivation of the adsorption sites.

[0004] In view of the fact that the selection of monomers and the specific synthesis method can affect the performance of polymer materials, it is urgent to provide a method for preparing a uranium adsorption material with high selectivity, large adsorption capacity and good environmental tolerance. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an aromatic oxime adsorption material and a preparation method and application thereof. The aromatic oxime adsorption material obtained by the preparation method provided by the present invention has the advantages of high selectivity, high adsorption efficiency and high adsorption capacity for uranium in seawater.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing an aromatic oxime adsorption material, comprising the following steps:

[0008] (1) Under an inert atmosphere, an aromatic diamine cyanide and an aprotic solvent a are mixed to obtain a solution A;

[0009] (2) under an inert atmosphere, mixing an aromatic cyanide dibasic acid anhydride, an acid-binding agent, and an aprotic solvent b to obtain a solution B;

[0010] (3) under an inert atmosphere, dropwise adding the solution A obtained in step (1) to the solution B obtained in step (2) to carry out an acylation reaction to obtain an amino-terminated polyamic acid oligomer;

[0011] (4) mixing the amino-terminated polyamic acid oligomer obtained in step (3) with a cross-linking agent to carry out a cross-linking reaction to obtain an adsorption material intermediate; the cross-linking agent is an aldehyde compound;

[0012] (5) mixing the adsorption material intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material;

[0013] There is no restriction on the order of step (1) and step (2).

[0014] Preferably, the aromatic diamine cyanide in step (1) has at least one of the chemical structures shown in formulas 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f, and the structural formulas of 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f are as follows:

[0015]

[0016] In the step (2), the aromatic cyaniding dibasic acid anhydride has at least one of the chemical structures shown in formulas 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F, and the structural formulas of 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F are as follows:

[0017]

[0018] Preferably, the aprotic solvent a in step (1) and the aprotic solvent b in step (2) are independently at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, methyl ethyl ketone, chlorobenzene, dimethyl sulfoxide, o-dichlorobenzene, dichloromethane, chloroform, 1,2-dichloroethane and ethyl acetate.

[0019] Preferably, the concentration of the aromatic cyanide diamine in solution A in step (1) is 0.1 to 6 mol / L; and the concentration of the aromatic cyanide dibasic acid anhydride in solution B in step (2) is 0.1 to 3.0 mol / L.

[0020] Preferably, in step (2), the acid binding agent comprises at least one of ethylamine, diethylamine, triethylamine, ethylenediamine, n-propylamine, n-butylamine, cyclohexylamine and N-methylaniline; and the molar ratio of the acid binding agent to the dibasic acid anhydride is 2.0:1 to 4.0:1.

[0021] Preferably, in step (3), the molar ratio of the aromatic cyaniding diamine in solution A to the aromatic cyaniding dibasic acid anhydride in solution B is 1.3:1 to 2.2:1.

[0022] Preferably, the temperature of the acylation reaction in step (3) is -20 to 0°C, the absolute pressure of the acylation reaction is 0 to 0.2 MPa, and the time of the acylation reaction is 8 to 14 hours.

[0023] Preferably, the aldehyde compound in step (4) comprises at least one of terephthalaldehyde, isophthalaldehyde, 2,5-furandicarboxaldehyde, 2,6-bipyridinecarboxaldehyde, 4,4'-biphenyldicarboxaldehyde and 3,4'-biphenyldicarboxaldehyde; and the molar ratio of the aldehyde compound to the aromatic diamine cyanide is 0.001:1 to 0.003:1.

[0024] The present invention also provides an aromatic oxime adsorption material prepared by the preparation method described in the above scheme.

[0025] The present invention also provides the use of the aromatic oxime adsorption material described in the above scheme in removing uranium from water.

[0026] The invention provides a method for preparing an aromatic oxime adsorption material, comprising the following steps: (1) mixing an aromatic cyanide diamine and an aprotic solvent a under an inert atmosphere to obtain a solution A; (2) mixing an aromatic cyanide dibasic acid anhydride, an acid-binding agent and an aprotic solvent b under an inert atmosphere to obtain a solution B; (3) dripping the solution A obtained in the step (1) into the solution B obtained in the step (2) under an inert atmosphere to carry out an acylation reaction to obtain an amino-terminated polyamic acid oligomer; (4) mixing the amino-terminated polyamic acid oligomer obtained in the step (3) with a crosslinking agent to carry out a crosslinking reaction to obtain an adsorption material intermediate; the crosslinking agent is an aldehyde compound; (5) mixing the adsorption material intermediate obtained in the step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material; there is no sequence restriction for steps (1) and (2). The present invention performs an acylation reaction on aromatic diamine cyanide and aromatic dibasic cyanide anhydride to obtain an amine-terminated oligomer, then performs a cross-linking reaction with a cross-linking agent to obtain an adsorbent intermediate, and finally performs an in-situ reduction reaction with hydroxylamine hydrochloride to finally obtain an aromatic oxime adsorbent. The present invention performs an acylation reaction on aromatic diamine cyanide and aromatic dibasic cyanide anhydride to obtain an amine-terminated oligomer with adjustable molecular scale, and then uses an aldehyde compound to cross-link it to obtain a uranium adsorbent with a specific "ion channel"; wherein the appropriate ion channel radius greatly improves the selectivity of the adsorbent; by selecting aromatic diamine cyanide and aromatic dibasic cyanide anhydride as reaction monomers, not only carboxyl groups and (secondary) amine groups are introduced into the adsorbent structure to enhance the hydrophilicity of the adsorbent surface, and the diffusion rate of uranyl at the interface is improved, but also aromatic rings are introduced, and the electronic conjugated structure of the aromatic rings effectively reduces the positive charge of the oxime carbon cation, hinders the attack of the oxime by the nucleophilic reagent, and improves the environmental tolerance of the adsorbent. Experimental results show that the aromatic oxime adsorption material prepared by the preparation method provided by the present invention exhibits good selectivity for uranium in seawater, and the adsorption capacity can reach 471.26 mg / g; after 10 cycles of adsorption and desorption, the adsorption capacity retention rate is greater than 98%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a pore size distribution diagram of the aromatic oxime adsorption material prepared in Example 1 of the present invention;

[0028] Figure 2 The physical image and scanning electron microscope image of the aromatic oxime adsorption material prepared in Example 1 of the present invention;

[0029] Figure 3 This is an isothermal adsorption curve of the aromatic oxime adsorption material prepared in Example 1 of the present invention;

[0030] Figure 4This is a graph showing the change in adsorption capacity of the aromatic oxime adsorption material prepared in Example 1 of the present invention after 10 cycles of adsorption and desorption;

[0031] Figure 5 This is a real seawater adsorption diagram of the aromatic oxime adsorption material prepared in Example 1 of the present invention;

[0032] Figure 6 This is a comparative column chart of the selectivity of the aromatic oxime adsorption material prepared in Example 1 of the present invention;

[0033] Figure 7 This is a Fourier infrared spectrum of the aromatic oxime adsorption material prepared in Example 1 and Example 2 of the present invention. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing an aromatic oxime adsorption material, comprising the following steps:

[0035] (1) Under an inert atmosphere, an aromatic diamine cyanide and an aprotic solvent a are mixed to obtain a solution A;

[0036] (2) under an inert atmosphere, mixing an aromatic cyanide dibasic acid anhydride, an acid-binding agent, and an aprotic solvent b to obtain a solution B;

[0037] (3) under an inert atmosphere, dropwise adding the solution A obtained in step (1) to the solution B obtained in step (2) to carry out an acylation reaction to obtain an amino-terminated polyamic acid oligomer;

[0038] (4) mixing the amino-terminated polyamic acid oligomer obtained in step (3) with a cross-linking agent to carry out a cross-linking reaction to obtain an adsorption material intermediate; the cross-linking agent is an aldehyde compound;

[0039] (5) mixing the adsorption material intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material;

[0040] There is no restriction on the order of step (1) and step (2).

[0041] In the present invention, aromatic cyanide diamine and aprotic solvent a are mixed under an inert atmosphere to obtain solution A.

[0042] In the present invention, the aromatic cyanide diamine preferably has at least one of the chemical structures shown in Formulas 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f, more preferably has one of the chemical structures shown in Formulas 1a, 2d, 3c and 4b, and most preferably has the chemical structure shown in Formula 1a.

[0043] In the present invention, the structural formulas of 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f are preferably as follows:

[0044]

[0045] The present invention selects the aromatic cyanide diamine of the structure to contain a cyano group, which is convenient for generating a group for capturing uranium, and at the same time contains an active functional group amino group that reacts with the aromatic cyanide dibasic acid anhydride; an aromatic ring is also introduced, and the electronic conjugation structure of the aromatic ring effectively reduces the positive charge of the oxime carbon cation, hinders the oxime group from being attacked by a nucleophilic reagent, and improves the environmental tolerance of the adsorption material.

[0046] In the present invention, the aprotic solvent a is preferably at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, methyl ethyl ketone, chlorobenzene, dimethyl sulfoxide, o-dichlorobenzene, dichloromethane, chloroform, 1,2-dichloroethane and ethyl acetate, and more preferably o-dichlorobenzene. The present invention selects the aprotic solvent a to dissolve the aromatic cyanide diamine, which can not only fully dissolve it, but also avoid the adverse effect of the solvent itself on the acylation reaction.

[0047] In the present invention, the concentration of the aromatic diamine cyanide in the solution A is preferably 0.1-6 mol / L, more preferably 0.2-2.0 mol / L. The present invention limits the concentration of the aromatic diamine cyanide in the solution A to the above range, and the resulting aromatic oxime adsorption material has good comprehensive performance.

[0048] In the present invention, the inert atmosphere gas when the aromatic diamine cyanide and the aprotic solvent a are mixed is preferably at least one of nitrogen, argon, helium and neon, more preferably argon or helium. The present invention prepares solution A under an inert atmosphere to prevent the active monomers of the aromatic diamine cyanide from being oxidized by air.

[0049] In the present invention, aromatic cyaniding dibasic acid anhydride, an acid-binding agent and aprotic solvent B are mixed under an inert atmosphere to obtain solution B.

[0050] In the present invention, the aromatic cyaniding dibasic acid anhydride preferably has at least one of the chemical structures shown in Formulas 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F, more preferably has a chemical structure shown in Formula 2B, 4E, 1D or 2F, and most preferably has a chemical structure shown in Formula 2B.

[0051] In the present invention, the structural formulas of 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F are preferably as follows:

[0052]

[0053] The present invention selects the aromatic cyanide dibasic acid anhydride of the above structure to contain a cyano group, which is convenient for generating a group that captures uranium, and at the same time contains an active functional group carboxyl group that reacts with the aromatic cyanide diamine, and also introduces an aromatic ring. The electronic conjugated structure of the aromatic ring effectively reduces the positive charge of the oxime carbon cation, hinders the oxime group from being attacked by a nucleophilic reagent, and improves the environmental tolerance of the adsorption material.

[0054] In the present invention, the aprotic solvent b is preferably at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, methyl ethyl ketone, chlorobenzene, dimethyl sulfoxide, o-dichlorobenzene, dichloromethane, chloroform, 1,2-dichloroethane and ethyl acetate, more preferably chlorobenzene.

[0055] The present invention selects the above-mentioned aprotic solvent b to dissolve the aromatic cyanided dibasic acid anhydride, which can not only fully dissolve the aromatic cyanided dibasic acid anhydride, but also prevent the solvent itself from having an adverse effect on the acylation reaction.

[0056] In the present invention, the concentration of the aromatic cyanide dibasic acid anhydride in solution B is preferably 0.1-3.0 mol / L, more preferably 0.2-2.5 mol / L. The present invention limits the concentration of the aromatic cyanide dibasic acid anhydride in solution B to the above range, and the resulting aromatic oxime adsorption material has good comprehensive performance.

[0057] In the present invention, the inert atmosphere gas when the aromatic cyaniding dibasic acid anhydride, the acid binding agent and the aprotic solvent b are mixed is preferably at least one of nitrogen, argon, helium and neon, more preferably argon or helium.

[0058] In the present invention, the mixing order of the aromatic cyaniding dibasic acid anhydride, the acid binding agent and the aprotic solvent b is preferably to first mix the aromatic cyaniding dibasic acid anhydride and the aprotic solvent b, and then to mix with the acid binding agent. In an embodiment of the present invention, the mixing of the aromatic cyaniding dibasic acid anhydride and the aprotic solvent b is preferably carried out under an argon atmosphere. In an embodiment of the present invention, the mixing of the acid binding agent is preferably carried out under a helium atmosphere. The embodiment of the present invention adopts a mixing method of first mixing the aromatic cyaniding dibasic acid anhydride and the aprotic solvent b under argon, and then mixing with the acid binding agent under a helium atmosphere, because the inert atmosphere gas in the solution preparation process in the laboratory is mainly provided by argon, and the inert gas in the reaction process is mainly provided by helium. The present invention mixes the aromatic cyaniding diamine and the aprotic solvent a, and the aromatic cyaniding dibasic acid anhydride and the aprotic solvent b, and prepares the required materials in advance; after adding the acid binding agent to the system of the aromatic cyaniding dibasic acid anhydride and the aprotic solvent b, the acylation reaction is carried out with the solution A.

[0059] In the present invention, solution B is prepared under an inert atmosphere, which can prevent the aromatic cyanide dibasic acid anhydride active monomer from being deliquesced by moisture in the air, thereby preventing the adverse effect on the acylation reaction.

[0060] After obtaining solution A and solution B, the present invention drips the solution A into the solution B to carry out acylation reaction, thereby obtaining an amino-terminated polyamic acid oligomer.

[0061] In the present invention, the ratio of the amount of aromatic cyanide diamine in solution A to the amount of aromatic cyanide dibasic acid anhydride in solution B is preferably 1.3:1 to 2.2:1, more preferably 1.5:1 to 2.0:1. The present invention limits the amount of aromatic cyanide diamine in solution A and aromatic cyanide dibasic acid anhydride in solution B to the above range, and the aromatic oxime adsorption material finally obtained has good comprehensive performance.

[0062] In the present invention, the acid binding agent preferably comprises at least one of ethylamine, diethylamine, triethylamine, ethylenediamine, n-propylamine, n-butylamine, cyclohexylamine and N-methylaniline, more preferably cyclohexylamine. In the present invention, the ratio of the amount of the acid binding agent to the amount of the aromatic cyaniding dibasic acid anhydride is preferably 2.0:1 to 4.0:1, more preferably 2.2:1 to 3.5:1. The present invention can increase the rate of the acylation reaction by selecting the above acid binding agent.

[0063] In the present invention, the temperature of the acylation reaction is preferably -20 to 0°C, more preferably -15 to 0°C; the absolute pressure of the acylation reaction is preferably 0 to 0.2 MPa, more preferably 0 to 0.1 MPa; the time of the acylation reaction is preferably 8 to 14 hours, more preferably 10 to 12 hours. In the present invention, the equipment for the acylation reaction is preferably a cold trap. The present invention has no special provisions on the specifications and materials of the cold trap, which can provide the temperature and pressure required for the acylation reaction.

[0064] In the present invention, the dropping rate is preferably 2 to 8 mmol / min, more preferably 3 to 7 mmol / min. The present invention controls the dropping rate within the above range to avoid excessive acylation reaction and improve the safety of the experiment.

[0065] In the present invention, the acylation reaction is preferably carried out under an inert atmosphere. In the present invention, the gas of the inert atmosphere is preferably at least one of nitrogen, argon, helium and neon, more preferably argon or helium. In the present invention, the acylation reaction is carried out under an inert atmosphere to avoid the adverse effects of oxygen and moisture in the air on the acylation reaction, thereby adversely affecting the aromatic oxime adsorption material finally prepared.

[0066] After obtaining the amino-terminated polyamic acid oligomer, the present invention mixes the amino-terminated polyamic acid oligomer and a cross-linking agent to carry out a cross-linking reaction to obtain an adsorption material intermediate.

[0067] In the present invention, the cross-linking agent is preferably an aldehyde compound. In the present invention, the aldehyde compound preferably includes at least one of terephthalaldehyde, isophthalaldehyde, 2,5-furandicarboxaldehyde, 2,6-bipyridinecarboxaldehyde, 4,4'-biphenyldicarboxaldehyde and 3,4'-biphenyldicarboxaldehyde, and is more preferably terephthalaldehyde. In the present invention, the amount ratio of the aldehyde compound to the aromatic diamine cyanide is preferably 0.001:1 to 0.003:1, and is more preferably 0.002:1. The present invention limits the type and amount of the cross-linking agent to the above range, and the comprehensive performance of the aromatic oxime adsorption material obtained is better.

[0068] In the present invention, the mixing of the amino-terminated polyamic acid oligomer and the crosslinking agent is preferably carried out under stirring. In the present invention, the stirring temperature is preferably room temperature. The present invention has no special provisions on the stirring rate, and stirring can be carried out at a stirring rate well known to those skilled in the art. The present invention mixes the amino-terminated polyamic acid oligomer and the crosslinking agent under stirring, which is conducive to sufficient crosslinking of the crosslinking agent and the amino-terminated polyamic acid oligomer, and obtains a uniformly mixed crosslinking system.

[0069] After the mixing is completed, the present invention preferably pours the mixed system immediately into a container for standing still, and then performs demoulding, soaking, washing and drying in sequence to obtain an adsorption material intermediate.

[0070] The present invention has no special provisions for the standing operation, and the standing operation familiar to those skilled in the art can be used. In the present invention, the standing container is preferably a watch glass. The present invention has no special provisions for the specifications of the watch glass, and a conventional selection can be used. The present invention has no special provisions for the standing time, and sufficient polymerization between the materials can be achieved. The present invention allows the polymer obtained by cross-linking the amino-terminated polyamic acid oligomer and the cross-linking agent to be more tightly cross-linked by standing in the watch glass.

[0071] The present invention has no special provisions for the demoulding operation. The demoulding operation well known to those skilled in the art can be used to separate the material after standing from the container used in the standing process.

[0072] In the present invention, the reagents used for the impregnation and washing are preferably at least one of water, methanol, glycerol and isopropanol, preferably one of water, methanol, glycerol and isopropanol. The present invention impregnates and washes the demoulded material, which is beneficial to the subsequent reduction reaction, thereby improving the comprehensive performance of the obtained aromatic oxime adsorption material.

[0073] The present invention has no special provisions for the impregnation operation. The impregnation operation well known to those skilled in the art can be used to fully impregnate the substance to be impregnated with the impregnation reagent.

[0074] The present invention has no special provisions for the washing operation, and the impurities on the impregnated material can be fully washed away by using a washing method well known to those skilled in the art.

[0075] The present invention has no special provisions on the drying method, drying temperature and drying time. A drying method well known to those skilled in the art can be used to fully dry and remove the washing agent on the washed material.

[0076] After obtaining the adsorption material intermediate, the present invention mixes the adsorption material intermediate, hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain the aromatic oxime adsorption material.

[0077] In the present invention, the solvent is preferably a mixture of water and methanol. In the present invention, the volume ratio of water to methanol is preferably (9-11):1, more preferably 10:1. In the present invention, the temperature of the reduction reaction is preferably 65-75°C, more preferably 70°C; the time of the reduction reaction is preferably 3-5h, more preferably 4h. The present invention limits the conditions of the reduction reaction to the above range, which is conducive to the full conduct of the reduction reaction.

[0078] The present invention has no special provisions on the mixing method. The material mixing method well known to those skilled in the art can be used to fully dissolve the reaction raw materials in the solvent.

[0079] The invention carries out acylation reaction on aromatic diamine cyanide and aromatic dibasic cyanide anhydride to obtain an amino-terminated oligomer with adjustable molecular scale, and cross-links the oligomer with an aldehyde compound to obtain a uranium adsorption material with a specific "ion channel". The suitable ion channel radius greatly improves the selectivity of the adsorbent. By selecting aromatic diamine cyanide and aromatic dibasic cyanide anhydride as reaction monomers, not only carboxyl groups and (secondary) amine groups are introduced into the intrinsic structure of the adsorbent to enhance the hydrophilicity of the adsorbent surface and improve the diffusion rate of uranyl at the phase interface, but also aromatic rings are introduced. The electronic conjugated structure of the aromatic rings effectively reduces the positive charge of the oxime carbon cation, hinders the attack of the oxime group by a nucleophilic reagent, and improves the environmental tolerance of the adsorbent.

[0080] The present invention also provides an aromatic oxime adsorption material prepared by the preparation method described in the above scheme. The aromatic oxime adsorption material provided by the present invention has the advantages of high selectivity and high adsorption capacity for uranium.

[0081] The present invention also provides the use of the aromatic oxime adsorption material described in the above scheme in the removal of uranium from water. The aromatic oxime adsorbent prepared by the preparation method provided by the present invention exhibits good selectivity for uranium in seawater, and the adsorption capacity can reach 471.26 mg / g; after 10 cycles of adsorption and desorption, the adsorption capacity retention rate is greater than 98%.

[0082] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0083] Example 1

[0084] A method for preparing an aromatic oxime adsorption material comprises the following steps:

[0085] (1) Under an argon atmosphere, 30 mmol of an aromatic diamine cyanide and 100 mL of an aprotic solvent, o-dichlorobenzene, were mixed to obtain a solution A having an aromatic diamine cyanide concentration of 0.3 mol / L;

[0086] The chemical structure of the aromatic diamine cyanide is shown in 1a:

[0087]

[0088] (2) Under an argon atmosphere, 20 mmol of an aromatic cyanide dibasic acid anhydride and 100 mL of an aprotic solvent, chlorobenzene, were first mixed, and then under a helium atmosphere, 40 mmol of an acid-binding agent, cyclohexylamine, was added to obtain a solution B having an aromatic cyanide dibasic acid anhydride concentration of 0.2 mol / L;

[0089] The chemical structure of the aromatic cyanide dibasic acid anhydride is shown in Formula 2B:

[0090]

[0091] (3) under a helium atmosphere, adding the solution A obtained in step (1) to the solution B obtained in step (2) at a rate of 3 mmol / min, and carrying out an acylation reaction in a cold trap at a temperature of -15°C and an absolute pressure of 0 MPa for 10 hours to obtain an amino-terminated polyamic acid oligomer;

[0092] Wherein, the ratio of the amount of aromatic cyanide diamine in solution A to the amount of aromatic cyanide dibasic acid anhydride in solution B is 1.5:1;

[0093] (4) under stirring at room temperature, 0.03 mmol of a crosslinking agent, terephthalaldehyde, and the amino-terminated polyamic acid oligomer obtained in step (3) are mixed to carry out a crosslinking reaction. After the crosslinking reaction is completed, the crosslinking reaction product is immediately poured into a 0.5 L surface dish and allowed to stand overnight. After demolding, the product is soaked in water, then washed with water, and then vacuum dried to obtain an adsorbent intermediate;

[0094] The ratio of the amount of crosslinking agent to the amount of aromatic diamine cyanide is 0.001:1;

[0095] (5) mixing the adsorbent intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent for reduction reaction to obtain an aromatic oxime adsorbent, which is referred to as adsorbent 1;

[0096] The solvent is a mixture of water and methanol, the volume ratio of water to methanol is 10:1, the reduction reaction temperature is 70°C, and the reaction time is 4h.

[0097] Example 2

[0098] A method for preparing an aromatic oxime adsorption material comprises the following steps:

[0099] (1) Under an argon atmosphere, 500 mmol of an aromatic diamine cyanide and 100 mL of an aprotic solvent, o-dichlorobenzene, were mixed to obtain a solution A having an aromatic diamine cyanide concentration of 5 mol / L;

[0100] The chemical structure of the aromatic diamine cyanide is shown in Formula 2d:

[0101]

[0102] (2) Under an argon atmosphere, 270 mmol of aromatic cyanide dibasic acid anhydride was first dissolved in 100 mL of aprotic solvent chlorobenzene, and then under a helium atmosphere, 702 mmol of acid-binding agent cyclohexylamine was added to obtain a solution B with a cyanide dibasic acid anhydride concentration of 2.7 mol / L;

[0103] The ratio of the amount of the acid-binding agent to the amount of the aromatic cyanide dibasic acid anhydride is 2.6:1.

[0104] The chemical structure of the aromatic cyanide dibasic acid anhydride is shown in Formula 4E:

[0105]

[0106] (3) under a helium atmosphere, adding the solution A obtained in step (1) to the solution B obtained in step (2) at a rate of 8 mmol / min, and carrying out an acylation reaction for 12 hours in a cold trap at a temperature of 0° C. and an absolute pressure of 0.1 MPa to obtain an amino-terminated polyamic acid oligomer;

[0107] Wherein, the ratio of the amount of aromatic cyanide diamine in solution A to the amount of aromatic cyanide dibasic acid anhydride in solution B is 1.9:1;

[0108] (4) under stirring conditions, 1.5 mmol of a crosslinking agent, terephthalaldehyde, and the amino-terminated polyamic acid oligomer obtained in step (3) are mixed to carry out a crosslinking reaction. After the mixing is completed, the mixed system is immediately poured into a 0.5 L watch glass dish and allowed to stand overnight. After demolding, the mixed system is soaked in methanol, then washed with methanol, and then vacuum dried to obtain an adsorbent intermediate;

[0109] Wherein, the ratio of the amount of the crosslinking agent to the amount of the aromatic diamine cyanide is 0.003:1;

[0110] (5) mixing the adsorbent intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent for reduction reaction to obtain an aromatic oxime adsorbent, which is referred to as adsorbent 2;

[0111] The solvent is a mixture of water and methanol, the volume ratio of water to methanol is 10:1, the reduction reaction temperature is 70°C, and the reaction time is 4h.

[0112] Example 3

[0113] A method for preparing an aromatic oxime adsorption material comprises the following steps:

[0114] (1) Under an argon atmosphere, 200 mmol of aromatic diamine cyanide was dissolved in 100 mL of an aprotic solvent, o-dichlorobenzene, to obtain a solution A having an aromatic diamine cyanide concentration of 2 mol / L;

[0115] The chemical structure of the aromatic diamine cyanide is shown in Formula 3c:

[0116]

[0117] (2) Under an argon atmosphere, 125 mmol of aromatic cyanide dibasic acid anhydride was first dissolved in 100 mL of aprotic solvent chlorobenzene, and then under a helium atmosphere, 375 mmol of an acid-binding agent cyclohexylamine was added to obtain a solution B having an aromatic cyanide dibasic acid anhydride concentration of 1.25 mol / L;

[0118] Wherein, the ratio of the amount of the acid binding agent to the amount of the aromatic cyanide dibasic acid anhydride is 3.0:1;

[0119] The chemical structure of the aromatic cyanide dibasic acid anhydride is shown in Formula 1D:

[0120]

[0121] (3) under a helium atmosphere, adding the solution A obtained in step (1) dropwise to the solution B obtained in step (2) at a rate of 6 mmol / min, and carrying out an acylation reaction for 11 hours in a cold trap at a temperature of -5°C and an absolute pressure of 0.05 MPa to obtain an amino-terminated polyamic acid oligomer;

[0122] Wherein, the ratio of the amount of aromatic cyanide diamine in solution A to the amount of aromatic cyanide dibasic acid anhydride in solution B is 1.6:1;

[0123] (4) under stirring at room temperature, 0.25 mmol of a crosslinking agent, terephthalaldehyde, and the amino-terminated polyamic acid oligomer obtained in step (3) are mixed for crosslinking reaction. After the mixing is completed, the mixed system is immediately poured into a 0.5 L surface dish and allowed to stand overnight. After demolding, the mixed system is soaked in glycerol, then washed with glycerol, and then vacuum dried to obtain an adsorbent intermediate;

[0124] Wherein, the ratio of the amount of the crosslinking agent to the amount of the aromatic diamine cyanide is 0.00125:1;

[0125] (5) mixing the adsorption material intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material;

[0126] The solvent is a mixture of water and methanol, the volume ratio of water to methanol is 10:1, the reduction reaction temperature is 70°C, and the reaction time is 4h.

[0127] Example 4

[0128] A method for preparing an aromatic oxime adsorption material comprises the following steps:

[0129] (1) Under an argon atmosphere, 80 mmol of an aromatic diamine cyanide was dissolved in 100 mL of an aprotic solvent, o-dichlorobenzene, to obtain a solution A having an aromatic diamine cyanide concentration of 0.8 mol / L;

[0130] The chemical structure of the aromatic diamine cyanide is shown in Formula 4b:

[0131]

[0132] (2) Under an argon atmosphere, 40 mmol of an aromatic cyanide dibasic acid anhydride was first dissolved in 100 mL of an aprotic solvent, chlorobenzene. Then, under a helium atmosphere, 128 mmol of an acid-binding agent, cyclohexylamine, was added to obtain a solution B having an aromatic cyanide dibasic acid anhydride concentration of 0.4 mol / L.

[0133] Wherein, the ratio of the amount of the acid binding agent to the amount of the aromatic cyanide dibasic acid anhydride is 3.2:1;

[0134] The chemical structure of the aromatic cyanide dibasic acid anhydride is shown in Formula 2F:

[0135]

[0136] (3) under a helium atmosphere, adding the solution A obtained in step (1) to the solution B obtained in step (2) at a rate of 4 mmol / min, and carrying out an acylation reaction for 10.5 h in a cold trap at a temperature of -10°C and an absolute pressure of 0.09 MPa to obtain an amino-terminated polyamic acid oligomer;

[0137] Wherein, the ratio of the amount of aromatic diamine cyanide in solution A to the amount of dibasic acid cyanide in solution B is 2:1;

[0138] (4) under stirring at room temperature, 0.16 mmol of a crosslinking agent, terephthalaldehyde, and the amino-terminated polyamic acid oligomer obtained in step (3) were mixed to carry out a crosslinking reaction. After the mixing was completed, the mixed system was immediately poured into a 0.5 L watch glass dish and allowed to stand overnight. After demolding, the mixed system was soaked in isopropanol, then washed with isopropanol, and then vacuum dried to obtain an adsorbent intermediate;

[0139] Wherein, the molar ratio of the crosslinking agent to the aromatic diamine cyanide is 0.002:1;

[0140] (5) mixing the adsorption material intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material;

[0141] The solvent is a mixture of water and methanol, the volume ratio of water to methanol is 10:1, the reduction reaction temperature is 70°C, and the reaction time is 4h.

[0142] Structural characterization

[0143] Taking Example 1 and Example 2 as examples, the aromatic oxime adsorption material prepared by the present invention was tested by Fourier transform infrared spectroscopy. The test results are shown in Figure 7 .Depend on Figure 7 It can be seen that at 1658cm -1 The characteristic absorption of amide I band appears at 15438 cm -1 NH characteristic bending vibration appears at 1543cm -1 The characteristic bending vibration of the hydroxyl group in the carboxyl group appears at 1500cm -1 , 835cm -1 , 1378cm -1 The characteristic skeleton of benzene ring, the characteristic absorption of benzene ring substitution and the stretching vibration of CN in the adsorbent appear at 1783 cm -1 The asymmetric stretching vibration of the ketone carbonyl group in the cyanide anhydride 4E is contained in the cyanide anhydride 4E. The existence of the above characteristic functional groups strongly proves the successful preparation of the adsorbent in the present invention.

[0144] Performance Testing

[0145] Uranium adsorption capacity test

[0146] First, a series of 250 mL uranium standard solutions of different concentrations (0 to 80 ppm, in terms of uranium element) were prepared with uranium nitrate hexahydrate. 10 mg of the adsorbent material prepared in the embodiment was accurately weighed and tested by static adsorption method. The uranium equilibrium concentration was recorded at equilibrium, the corresponding adsorption amount was calculated and a related curve was drawn. The relevant models such as Langmuir (Formula 1) and Freundlich (Formula 2) were fitted, and the adsorption capacity was calculated using the model with higher fitting degree.

[0147]

[0148]

[0149] Among them, C e (mg / L) and q e (mg / g) is the concentration of uranium in the solution and the corresponding adsorption amount of the adsorbent when adsorption equilibrium is reached; q m (mg / g) is the adsorption capacity; k L (L / mg) is the Langmuir adsorption constant; k F and n is the Freundlich adsorption constant.

[0150] Desorption process: The adsorbent is placed in a mixture of 1 mol / L sodium carbonate and 0.1 mol / L hydrogen peroxide and stirred for a period of time. After the desorption is completed, the uranium content of the adsorbent is determined by an inductively coupled plasma mass spectrometer, and then the next adsorption process is entered.

[0151] Figure 1 This is a microscopic pore size distribution diagram of the aromatic oxime adsorbent material prepared in Example 1 of the present invention. It can be seen from the figure that the microscopic pore size of the aromatic oxime adsorbent material is Slightly larger than the radius of uranyl ions in seawater, this specific pore structure improves the selectivity of the adsorption material.

[0152] Figure 2 A physical picture of the aromatic oxime adsorption material prepared in Example 1 of the present invention ( Figure 2 A), Field emission scanning electron microscope cross-section ( Figure 2 B: cross-sectional macroscopic image; Figure 2 C: Cross-section magnified at 100,000 times;

[0153] Figure 2D: 200,000 magnified cross-section). As can be seen from the figure, the aromatic oxime adsorbent material has a uniform appearance, and the SEM magnified image shows a uniform open pore structure. The pores are generated by the exchange of aromatic oxime intermediates between the detergent and the reaction solvent during the washing process. The porous structure of the adsorbent provides an "ion channel" for the rapid diffusion of uranyl ions to the interface containing multiple active sites.

[0154] Figure 3 The isothermal adsorption curve of the aromatic oxime adsorption material prepared in Example 1 of the present invention shows that the adsorption process conforms to the Langmuir isothermal adsorption model and is a monolayer uniform adsorption. According to calculations, the maximum adsorption capacity of the adsorption material prepared by the inventive method reaches 471.26 mg / g.

[0155] Figure 4 This is a graph showing the change in adsorption capacity of the aromatic oxime adsorption material prepared in Example 1 of the present invention after 10 cycles of adsorption and desorption. Figure 4 It can be seen that after a long period of adsorption and desorption cycles, the adsorption capacity of the adsorbent remains above 98%, highlighting the good environmental tolerance of aromatic oxime adsorption materials. The reason for the high adsorption capacity retention rate is that the oxime carbon cation forms a conjugated structure with the electrons on the benzene ring, which effectively hinders the attack of the carbon cation by nucleophilic reagents and improves the structural stability of the oxime derivatives.

[0156] Figure 5 The adsorption kinetic curve of uranium by the aromatic oxime adsorption material prepared in Example 1 of the present invention placed in natural sea areas. Figure 5 It can be seen that after 12 days of adsorption, the adsorption amount of aromatic oxime adsorption material can reach 8.42 mg, and the adsorption rate is 0.701 mg g1 day1, which is a relatively high level reported in the research.

[0157] Figure 6 This is a comparison chart of the adsorption energy absorption of common competitive molecules in seawater by the aromatic oxime adsorption material prepared in Example 1 of the present invention. (From left to right, divalent, divalent, divalent, trivalent, divalent, pentavalent, divalent and all positive, provided by the corresponding nitrates), Figure 6 It can be seen that the aromatic oxime adsorption material prepared by the method of the invention has good selectivity, overcoming the disadvantage of poor selectivity of traditional oxime-based adsorbents for vanadium, iron, etc.

[0158] The above experiments prove that the aromatic oxime adsorption material prepared by the preparation method provided by the present invention has the advantages of high selectivity, large adsorption capacity and good environmental tolerance.

[0159] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an aromatic oxime adsorption material, The following steps are involved: (1) Under an inert atmosphere, an aromatic diamine cyanide and an aprotic solvent a are mixed to obtain a solution A; (2) under an inert atmosphere, mixing an aromatic cyanide dibasic acid anhydride, an acid-binding agent, and an aprotic solvent b to obtain a solution B; (3) under an inert atmosphere, adding the solution A obtained in step (1) dropwise to the solution B obtained in step (2) to carry out an acylation reaction to obtain an amino-terminated polyamic acid oligomer; the acylation reaction temperature is -20 to 0° C., the acylation reaction absolute pressure is 0 to 0.2 MPa, and the acylation reaction time is 8 to 14 h; (4) mixing the amino-terminated polyamic acid oligomer obtained in step (3) with a cross-linking agent to carry out a cross-linking reaction to obtain an adsorption material intermediate; the cross-linking agent is an aldehyde compound; (5) mixing the adsorption material intermediate obtained in step (4), hydroxylamine hydrochloride and a solvent to carry out a reduction reaction to obtain an aromatic oxime adsorption material; There is no order restriction for step (1) and step (2); In the step (1), the aromatic diamine cyanide has at least one of the chemical structures shown in formulas 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f, and the structural formulas of 1a to 1e, 2a to 2f, 3a to 3f and 4a to 4f are as follows: In the step (2), the aromatic cyaniding dibasic acid anhydride has at least one of the chemical structures shown in formulas 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F, and the structural formulas of 1A to 1D, 2A to 2F, 3A to 3F and 4A to 4F are as follows:

2. The preparation method according to claim 1, It is characterized in that The aprotic solvent a in step (1) and the aprotic solvent b in step (2) are independently at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, methyl ethyl ketone, chlorobenzene, dimethyl sulfoxide, o-dichlorobenzene, dichloromethane, chloroform, 1,2-dichloroethane and ethyl acetate.

3. The preparation method according to claim 1, It is characterized in that In the step (1), the concentration of the aromatic cyaniding diamine in solution A is 0.1 to 6 mol / L; and in the step (2), the concentration of the aromatic cyaniding dibasic acid anhydride in solution B is 0.1 to 3.0 mol / L.

4. The preparation method according to claim 1, It is characterized in that In the step (2), the acid-binding agent comprises at least one of ethylamine, diethylamine, triethylamine, ethylenediamine, n-propylamine, n-butylamine, cyclohexylamine and N-methylaniline; and the molar ratio of the acid-binding agent to the aromatic cyaniding dibasic acid anhydride is 2.0:1 to 4.0:

1.

5. The preparation method according to claim 1, It is characterized in that In the step (3), the molar ratio of the aromatic cyaniding diamine in solution A to the aromatic cyaniding dianhydride in solution B is 1.3:1 to 2.2:

1.

6. The preparation method according to claim 1, It is characterized in that The aldehyde compound in step (4) includes at least one of terephthalaldehyde, isophthalaldehyde, 2,5-furandicarboxaldehyde, 2,6-dipyridinecarboxaldehyde, 4,4'-biphenyldicarboxaldehyde and 3,4'-biphenyldicarboxaldehyde; the amount ratio of the aldehyde compound to the aromatic diamine cyanide is 0.001:1 to 0.003:

1.

7. The aromatic oxime adsorption material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the aromatic oxime adsorption material according to claim 7 in removing uranium from water.