A method for regenerating anthraquinone degradation products, a regeneration catalyst and its preparation

By using composite catalysts of alumina, magnesium oxide and transition metal oxides, the shortcomings of existing alumina catalysts in the regeneration of anthraquinone degradable substances are solved, and efficient regeneration and recycling rate are improved, and production costs are reduced.

CN115999528BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202111232178.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-22
Publication Date
2024-11-12
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

The existing alumina and modified alumina as anthraquinone degradation regeneration catalysts have problems such as inability to completely regenerate partial degradation, insufficient mechanical strength, easy powdering and unfriendly environment, resulting in low regeneration efficiency and high production costs.

Method used

Using a composite catalyst with aluminum oxide, magnesium oxide, fluoride and transition metal oxide as the main components, the soluble aluminum salt and magnesium salt are precipitated, filtered and dried in an alkaline solution, and combined with a binder to form a spherical catalyst. Improve the strength and life of the catalyst.

Benefits of technology

The regeneration efficiency of anthraone type, hydroxyanthraone and tetrahydroanthraquinone epoxide is significantly improved, the use cycle of the catalyst is extended, the production cost is reduced, and the recycling rate of the working liquid is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115999528B_ABST
    Figure CN115999528B_ABST
Patent Text Reader

Abstract

The invention discloses an anthraquinone degradation product regeneration catalyst, characterized in that, based on dry basis and based on the weight of the catalyst, the catalyst comprises 10-98 weight percent of aluminum oxide, 1-80 weight percent of magnesium oxide, 1-30 weight percent of fluoride and 0-10 weight percent of transition metal oxide selected from Group VIB and Group VIIB. The catalyst can greatly increase the total amount of effective anthraquinone and effectively improve the recycling rate of the working fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the regeneration of anthraquinone degradation products in the technical field of producing hydrogen peroxide by anthraquinone method, a metal-containing regeneration catalyst and a preparation method of the regeneration catalyst. Background Art

[0002] Hydrogen peroxide (its aqueous solution is called hydrogen peroxide) has the molecular formula of H2O2. It is a strong oxidant that can be mixed with water in any ratio and is widely used in the fields of chemical industry, papermaking, printing and dyeing, and environmental protection. In recent years, hydrogen peroxide has been widely used in the production of bulk chemicals such as caprolactam and propylene oxide, and its output and usage have grown rapidly.

[0003] The anthraquinone method is the main method for producing hydrogen peroxide in industry at present. The anthraquinone method for producing hydrogen peroxide is a process in which a working carrier is dissolved in an organic solvent to form a working liquid, and the working liquid undergoes a hydrogenation process, an oxidation process, and an extraction process to obtain hydrogen peroxide. The working carrier for producing hydrogen peroxide by the anthraquinone method can be alkyl anthraquinone and / or hydrogenated alkyl anthraquinone, and the organic solvent is generally a mixed solvent of heavy aromatic hydrocarbons and esters or higher alcohols. In the hydrogenation process, the working carrier is hydrogenated with H2 in the presence of a hydrogenation catalyst to generate the corresponding alkyl hydroanthraquinone and / or hydrogenated alkyl hydroanthraquinone to obtain a hydrogenated liquid; in the oxidation process, the hydrogenated liquid is contacted with oxygen or air to generate hydrogen peroxide, and the alkyl hydroanthraquinone and / or hydrogenated alkyl hydroanthraquinone are restored to alkyl anthraquinone and / or hydrogenated alkyl anthraquinone; in the extraction process, hydrogen peroxide is extracted from the oxidation liquid with water, and the raffinate is recycled to the hydrogenation process after post-treatment.

[0004] In the process of producing hydrogen peroxide by anthraquinone method, some side reactions will occur in the hydrogenation process and oxidation process, resulting in degradation of the working carrier, making it lose the ability to produce hydrogen peroxide, and forming useless inert degradation products, such as octahydroanthraquinone, hydroxyanthraquinone, anthraquinone, tetrahydroanthraquinone epoxide, etc., among which anthraquinone is the most important inert degradation product. The generation of inert degradation products not only reduces the anthraquinone content in the working solution, reduces the preparation efficiency of hydrogen peroxide, but also causes changes in the physical properties of the working solution, such as surface tension decrease, viscosity increase, system resistance increase, effective component loss, etc., which ultimately lead to a decrease in hydrogen peroxide yield, quality decrease, and increased production cost, making the process unable to proceed normally. Therefore, the regeneration of anthraquinone degradation products has always been the focus of people's attention and research. At present, white clay (basic alumina) is widely used in industry to regenerate degradation products. Due to the relatively complex composition of the working solution and the degradation mechanism of anthraquinone, there are many types of degradation products generated, so it is difficult to find a regeneration catalyst to convert all degradation products into effective anthraquinone. The commonly used white clay in industry can only regenerate certain degradation products, with low regeneration efficiency. Moreover, fresh white clay must be frequently replaced to maintain stable production. Each replacement of white clay will cause loss of working fluid, which undoubtedly increases labor intensity and production costs. Therefore, it is of great significance to develop catalysts with high regeneration efficiency.

[0005] USP0018013 discloses a catalyst for regenerating anthraquinone degradation products in the H2O2 industry and a method for preparing the same. The invention first immerses alumina in a saturated aqueous solution of a magnesium salt, then uses an ammonia solution with a pH of 9-13 to precipitate magnesium ions in the alumina pores, and finally roasts at 300-800°C to obtain 1-50% MgO / Al2O3. The method is improved on the basis of the traditional anthraquinone degradation product regeneration catalyst and has certain application value. However, since MgO reacts with water in the anthraquinone working solution to generate hexagonal flaky Mg(OH)2 with a particle size of about 2-3μm. Therefore, after the MgO undergoes a crystal phase change in the alumina pores, the particle size changes significantly, which will generate stress that breaks the alumina pores, reduce the crushing strength of the catalyst, shorten the service life, and have a serious impact on the production of hydrogen peroxide.

[0006] USP4668499 discloses a method of using aromatic tertiary amine as a catalyst for regenerating degradation products in an oxygen atmosphere. The catalyst is a homogeneous catalyst and can be recycled together with the working fluid. It mainly regenerates degradation products produced by excessive hydrogenation. However, the types of regenerable degradation products of the catalyst are relatively small, the regeneration efficiency is low, and it is not easy to separate and recover. In addition, the stability of aromatic tertiary amine under harsh anthraquinone hydrogenation and oxidation conditions remains to be investigated.

[0007] CN102728338A provides an anthraquinone degradation product regeneration catalyst which can be expressed as MeO / Al2O3, wherein MeO is any one or more of an alkaline earth metal oxide or ZnO. The catalyst has a relatively high regeneration efficiency, but since a hydrotalcite precursor needs to be synthesized by a hydrothermal method during preparation, the preparation process is complicated and the preparation cost of the catalyst is relatively high.

[0008] CN106540685A and CN 106629620A provide a method for preparing an alumina-supported anthraquinone degradation product regeneration catalyst containing at least one ⅡA metal element and at least one second metal element and a method for regenerating a working solution. The catalyst has a good regeneration effect on anthrone degradation products, but the regeneration effect on other types of degradation products such as hydroxyanthraquinone and tetrahydroanthraquinone epoxide is not mentioned.

[0009] At present, alumina and modified alumina have many shortcomings as anthraquinone degradation product regeneration catalyst: (1) only part of the degradation product can be regenerated, and the regeneration of the degradation product is not thorough enough; (2) the mechanical strength of alumina is not enough, and it is easy to pulverize in the alkaline working solution, which will increase the burden of alkali separation in the post-treatment process; (3) the system often has water and alkali phenomena during regeneration, which has a certain impact on production. Although people have proposed to increase the life of the regenerated catalyst by adding other solid alkali compounds such as Mg, this type of regenerated catalyst is often prepared using nitrate as a precursor salt, and the preparation process is not environmentally friendly. For example, the roasting process will produce a large amount of nitrogen oxides that pollute the environment; at the same time, due to the limited solubility of Mg(NO3)2·6H2O in water, when preparing high-load solid alkali, it is often necessary to use high temperature and multiple impregnation methods to complete it, which greatly increases the manufacturing cost. Summary of the invention

[0010] In view of the problems existing in the prior art, the purpose of the present invention is to provide an anthraquinone degradation product regeneration catalyst which is composited with multiple base strengths and can efficiently regenerate different types of degradation products, and to provide a preparation method and application thereof.

[0011] In order to achieve the above-mentioned object, the first aspect of the present invention provides an anthraquinone degradation product regeneration catalyst, characterized in that, calculated on a dry basis and based on the weight of the catalyst, the catalyst comprises 10-98 weight % of aluminum oxide, 1-80 weight % of magnesium oxide, 1-30 weight % of fluoride and 0-10 weight % of an oxide of a transition metal M selected from Group VIB and Group VIIB.

[0012] In order to achieve the above object, the second aspect of the present invention also provides a method for preparing anthraquinone degradation product regeneration catalyst, characterized in that the method comprises the steps of:

[0013] (1) dissolving a soluble aluminum salt, a soluble magnesium salt and an optionally added soluble compound of a transition metal M selected from Group VIB and / or Group VIIB in deionized water to prepare a mixed salt solution;

[0014] (2) adding an alkaline solution to the mixed salt solution to form a precipitate, filtering after the precipitation is complete, washing with water until the pH value is 11-12, and drying to obtain a powder;

[0015] (3) The powder obtained in (2), fluoride and a binder are fully mixed and molded.

[0016] In order to achieve the above-mentioned object, the third aspect of the present invention further provides a method for regenerating a circulating working liquid in the production of hydrogen peroxide by anthraquinone method, comprising contacting the circulating working liquid with the anthraquinone degradation product regeneration catalyst provided by the present invention or the anthraquinone degradation product regeneration catalyst obtained by the preparation method of the present invention, so that the anthraquinone type, hydroxyanthraquinone, tetrahydroanthraquinone epoxide and tetrahydro-2-alkylanthraquinone compounds in the circulating working liquid are converted into anthraquinone type compounds.

[0017] The anthraquinone degradation product regeneration catalyst provided by the present invention significantly improves the ability of converting anthraquinone-type, hydroxyanthraquinone, tetrahydroanthraquinone epoxide and tetrahydro-2-alkylanthraquinone compounds in the circulating working fluid into effective anthraquinone-type compounds, greatly increases the total amount of effective anthraquinone, and effectively improves the recycling rate of the working fluid. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the TPD-CO2 spectrum of the regenerated catalyst-1 prepared in Example 1.

[0019] Figure 2 This is the TPD-CO2 spectrum of the white clay used in Comparative Test Example 2. DETAILED DESCRIPTION

[0020] A catalyst for regenerating anthraquinone degradation products, characterized in that, on a dry basis and based on the weight of the catalyst, the catalyst comprises 10-98 wt % of aluminum oxide, 1-80 wt % of magnesium oxide, 1-30 wt % of fluoride and 0-10 wt % of an oxide of a transition metal M selected from Group VIB and Group VIIB.

[0021] Preferably, the catalyst comprises 30-92 wt% of aluminum oxide, 2-10 wt% of fluoride, 5-67 wt% of magnesium oxide and 0.2-8 wt% of oxide of transition metal M selected from Group VIB and Group VIIB. More preferably, the catalyst comprises 48-72 wt% of aluminum oxide, 4-8 wt% of fluoride, 10-40 wt% of magnesium oxide and 1-6 wt% of oxide of transition metal M selected from Group VIB and Group VIIB.

[0022] The fluoride is preferably calcium fluoride, magnesium fluoride or aluminum fluoride. The oxide of the transition metal M of group VIB is preferably molybdenum oxide or chromium oxide, and the oxide of the transition metal M of group VIIB is preferably manganese oxide.

[0023] The regenerated catalyst is characterized in that the TPD-CO2 spectrum of the catalyst has three main peaks, which respectively represent the weak alkaline position of about 100°C, the medium alkaline position of 306°C and the strong alkaline position of 660°C of the oxide.

[0024] The regenerated catalyst can be formed into a spherical catalyst with a particle size of 0.5 to 5.0 mm and has a strength of 120 N / particle to 190 N / particle, preferably 135 N / particle to 170 N / particle.

[0025] The present invention also provides a method for preparing anthraquinone degradation product regeneration catalyst, characterized in that the method comprises the steps of:

[0026] (1) dissolving a soluble aluminum salt, a soluble magnesium salt and an optionally added soluble compound of a transition metal M selected from Group VIB and / or Group VIIB in deionized water to prepare a mixed salt solution;

[0027] (2) adding an alkaline solution to the mixed salt solution to form a precipitate, filtering after the precipitation is complete, washing with water until the pH value is 11-12, and drying to obtain a powder;

[0028] (3) The powder obtained in (2), fluoride and a binder are fully mixed and molded.

[0029] In the preparation method, step (1) further comprises ultrasonic oscillation at 30-90° C. for 1-12 h after the precipitation is complete.

[0030] In the preparation method, the fluoride is a mixture of one or more of CaF2, MgF2 and AlF3. The alkaline solution is selected from a mixture of one or more of NaOH, KOH, Na2CO3, NaHCO3 or ammonia water. The VIB group and / or VIIB group transition metal M is selected from at least one of tungsten, molybdenum, chromium and manganese. The soluble compound of the VIB group and VIIB group transition metal M is one or more of sodium tungstate, ammonium tungstate, sodium molybdate, ammonium molybdate, chromium nitrate and manganese nitrate.

[0031] The binder binds the oxide powder particles containing the aluminum carrier and MgO and the transition metal M together to improve the strength and life of the composite catalyst. When the amount of binder added is insufficient, it is difficult to form, and even if it is barely formed, it will break when leaving the molding machine. When the amount of binder is too much, the spherical product becomes soft and sticky. In the present invention, the binder can be selected from at least one of aluminum sol, silica sol and water glass, and the preferred binder is aluminum sol. If silica sol is used as the binder, it can be acidic silica sol or alkaline silica sol, which can be commercially available or prepared according to any prior art. Other inorganic oxide precursors with bonding effects known to those skilled in the art can also be added during the preparation of the composite catalyst.

[0032] Preferably, the molding is to obtain a spherical catalyst with a particle size of 0.5 to 5.0 mm through a molding process. An optional molding process is to roll the catalyst into small balls in a ball rolling machine, sieve out small balls with a diameter of 0.5 to 5.0 mm from the obtained small balls, dry and calcine them to obtain small balls. The small ball catalyst can be used in a fixed bed reactor or a moving bed reactor.

[0033] In the method provided by the present invention, the catalyst precursor after ball forming can be dried and calcined to improve the catalyst strength. The drying and calcination are well known to those skilled in the art. For example, the drying conditions may include: a temperature of 80-200°C and a time of 1-10h, and the calcination conditions may include: a temperature of 200-900°C and a time of 0.5-10h.

[0034] The present invention further provides a catalyst for regenerating anthraquinone degradation products obtained by the above preparation method.

[0035] The present invention further provides a method for regenerating a circulating working fluid in the production of hydrogen peroxide by anthraquinone method, comprising contacting the circulating working fluid with the anthraquinone degradation product regeneration catalyst provided by the present invention or the anthraquinone degradation product regeneration catalyst obtained by the preparation method provided by the present invention, so that the anthraquinone type, hydroxyanthraquinone, tetrahydroanthraquinone epoxide and tetrahydro-2-alkylanthraquinone compounds in the circulating working fluid are converted into anthraquinone type compounds.

[0036] The regeneration method of the circulating working fluid, wherein the circulating working fluid contacts the regenerated catalyst under the conditions of a temperature of 20-120°C and a pressure of 0-1.5MPa, wherein the pressure is a gauge pressure. Preferably, the regeneration method, wherein the temperature is 30-90°C and the pressure is 0-1MPa. The preferred regeneration method is carried out in a fixed bed or moving bed reactor, and the circulating working fluid weight hourly space velocity is 1-100h -1 .

[0037] The present invention is further described below through specific implementation modes. It should be understood that the specific implementation modes described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0038] In the following examples and comparative examples, the composition of the working solution and the regenerated working solution was analyzed by liquid chromatography, and the liquid chromatography analysis was performed on an Agilent 1260LC liquid chromatograph equipped with a C18 reverse phase chromatography column.

[0039] In the following examples and comparative examples, X-ray fluorescence spectroscopy was used to determine the composition of the catalyst.

[0040] The TPD-CO2 properties of the catalyst and clay in the examples and comparative examples were characterized by using an Autochem 2950 chemical adsorption instrument produced by Micromeritic. The test process is as follows: weigh about 0.1 g of sample into a U-shaped sample tube and place it in a heating furnace; introduce helium and heat it to 350°C for 1 hour; then cool the sample to 50°C, introduce carbon dioxide after the baseline is stable, and after adsorption saturation, purge with helium for 1 hour until the baseline is stable; finally, heat the sample to 800°C at a rate of 15°C / min for programmed temperature desorption.

[0041] The catalyst strength in the examples was measured using a DL3 intelligent particle strength tester produced by Dalian Penghui Technology Development Co., Ltd. Measurement method: Randomly test the crushing force values ​​of 150 spherical particles and take the average value, in N.

[0042] In the following examples, unless otherwise specified, all reagents used are commercially available reagents.

[0043] In the following examples and comparative examples, unless otherwise specified, pressures are gauge pressures.

[0044] Examples 1-7 illustrate the regenerated catalysts of the present invention and methods for their preparation.

[0045] Example 1

[0046] (1) At room temperature, 128 g of Mg(NO3)2·6H2O and 375 g of Al(NO3)3·9H2O were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0047] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0048] (3) The mixed powder obtained in (2) was fully mixed with 5g CaF2 and 30g aluminum sol (a product of Hunan Jucheng Co., Ltd., containing 21.5% by weight of Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were screened out from the obtained pellet catalyst, and dried at 120°C for 4 hours. Finally, the sample was placed in a muffle furnace, programmed to heat to 550°C, and calcined at a constant temperature for 4 hours to obtain spherical catalyst-1. The catalyst strength was measured by a strength tester and was 140N / pellet.

[0049] Catalyst-1 consists of 69.7 wt% Al2O3, 6.1 wt% calcium fluoride and 24.2 wt% MgO.

[0050] Figure 1 The TPD-CO2 spectrum of catalyst-1 is shown in the figure. As can be seen from the figure, the TPD-CO2 spectrum of catalyst-1 shows three main peaks, namely the weak alkaline position of the oxide (~100℃), a medium-strong alkaline position (306℃) and a strong alkaline position (660℃). White clay only has one medium-strong alkaline position (286℃).

[0051] Example 2

[0052] (1) At room temperature, 128 g of Mg(NO3)2·6H2O, 375 g of Al(NO3)3·9H2O and 10 g of 50% manganese nitrate aqueous solution were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0053] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0054] (3) The mixed powder obtained in (2) was fully mixed with 5g CaF2 and 30g aluminum sol (a product of Hunan Jucheng Co., Ltd., containing 21.5% by weight of Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were screened out from the obtained pellet catalyst, and dried at 120°C for 4 hours. Finally, the sample was placed in a muffle furnace, programmed to rise to 550°C, and calcined at a constant temperature for 4 hours to obtain spherical catalyst-2. The catalyst strength was measured by a strength tester and was 146N / pellet.

[0055] Catalyst-2 consists of 65.8 wt% Al2O3, 5.7 wt% calcium fluoride, 5.6 wt% MnO2 and 22.9 wt% MgO.

[0056] The TPD-CO2 spectrum of catalyst-2 has Figure 1 characteristics.

[0057] Example 3

[0058] (1) At room temperature, 128 g of Mg(NO3)2·6H2O, 375 g of Al(NO3)3·9H2O and 10 g of chromium nitrate were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0059] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0060] (3) The mixed powder obtained in (2) was fully mixed with 5g CaF2 and 30g aluminum sol (Hunan Jucheng Co., Ltd. product, containing 21.5 wt% Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were sieved out from the obtained pellet catalyst, and dried at 120°C for 4h. Finally, the sample was placed in a muffle furnace, programmed to 550°C, and calcined at a constant temperature for 4h to obtain spherical catalyst-3. The catalyst strength was measured by a strength tester and was 160N / pellet.

[0061] Catalyst-3 consists of 68.1 wt% Al2O3, 5.9 wt% calcium fluoride, 2.3 wt% Cr2O3 and 23.7 wt% MgO.

[0062] The TPD-CO2 spectrum of catalyst-3 has Figure 1 characteristics.

[0063] Example 4

[0064] (1) At room temperature, 128 g of Mg(NO3)2·6H2O and 187.5 g of Al(NO3)3·9H2O were dissolved in 600 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:1, and the solution was placed in a constant temperature water bath at 40°C;

[0065] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0066] (3) The mixed powder obtained in (2) was fully mixed with 5g CaF2 and 30g aluminum sol (Hunan Jucheng Co., Ltd. product, containing 21.5 wt% Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were sieved out from the obtained pellet catalyst, and dried at 120°C for 4h. Finally, the sample was placed in a muffle furnace, programmed to 550°C, and calcined at a constant temperature for 4h to obtain spherical catalyst-4. The catalyst strength was measured by a strength tester and was 170N / pellet.

[0067] Catalyst-4 consists of 56.1 wt% Al2O3, 8.8 wt% calcium fluoride and 35.1 wt% MgO.

[0068] The TPD-CO2 spectrum of catalyst-4 has Figure 1 characteristics.

[0069] Example 5

[0070] (1) At room temperature, 128 g of Mg(NO3)2·6H2O and 375 g of Al(NO3)3·9H2O were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0071] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0072] (3) The mixed powder obtained in (2) was fully mixed with 5g MgF2 and 30g aluminum sol (a product of Hunan Jucheng Co., Ltd., containing 21.5% by weight of Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were screened out from the obtained pellet catalyst, and dried at 120°C for 4 hours. Finally, the sample was placed in a muffle furnace, programmed to heat up to 550°C, and calcined at a constant temperature for 4 hours to obtain spherical catalyst-5. The catalyst strength was measured by a strength tester and was 162N / pellet.

[0073] Catalyst-5 consists of 69.7 wt% Al2O3, 6.1 wt% magnesium fluoride and 24.2 wt% MgO.

[0074] The TPD-CO2 spectrum of catalyst-5 has Figure 1 characteristics.

[0075] Example 6

[0076] (1) At room temperature, 128 g of Mg(NO3)2·6H2O, 375 g of Al(NO3)3·9H2O and 5 g of ammonium molybdate were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0077] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0078] (3) The mixed powder obtained in (2) was fully mixed with 5g CaF2 and 30g aluminum sol (a product of Hunan Jucheng Co., Ltd., containing 21.5% by weight of Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were screened out from the obtained pellet catalyst, and dried at 120°C for 4 hours. Finally, the sample was placed in a muffle furnace, programmed to heat up to 550°C, and calcined at a constant temperature for 4 hours to obtain spherical catalyst-6. The catalyst strength was measured by a strength tester and was 146N / pellet.

[0079] Catalyst-6 consists of 66.4 wt% Al2O3, 5.8 wt% calcium fluoride, 4.7 wt% MoO3 and 23.1 wt% MgO.

[0080] The TPD-CO2 spectrum of catalyst-6 has Figure 1 characteristics.

[0081] Example 7

[0082] (1) At room temperature, 128 g of Mg(NO3)2·6H2O and 375 g of Al(NO3)3·9H2O were dissolved in 700 mL of deionized water to prepare a mixed salt solution of magnesium nitrate and aluminum nitrate with a molar ratio of magnesium to aluminum of 1:2, and the solution was placed in a constant temperature water bath at 40°C;

[0083] (2) adding 20% ​​NaOH solution dropwise to the mixed salt solution, adjusting the pH value of the mixed solution to maintain at 11-13, and after precipitation is complete, continuing ultrasonic oscillation at 60°C for 2 hours; filtering, washing with hot water until the pH value is 7, and drying at 110°C for 12 hours; placing the dried powder in a muffle furnace and calcining at 500-800°C for 4 hours;

[0084] (3) The mixed powder obtained in (2) was fully mixed with 5g AlF3 and 30g aluminum sol (a product of Hunan Jucheng Co., Ltd., containing 21.5% by weight of Al2O3), and rolled into a pellet catalyst in a BY-800 water chestnut-type rolling ball machine (Taizhou Tiantai Pharmaceutical Machinery Factory). The pellets with a diameter of 0.5 to 5.0 mm were screened out from the obtained pellet catalyst, and dried at 120°C for 4 hours. Finally, the sample was placed in a muffle furnace, programmed to heat up to 550°C, and calcined at a constant temperature for 4 hours to obtain spherical catalyst-7. The catalyst strength was measured by a strength tester and was 138N / pellet.

[0085] Catalyst-7 consists of 69.7 wt% Al2O3, 6.1 wt% aluminum fluoride and 24.2 wt% MgO.

[0086] The TPD-CO2 spectrum of catalyst-7 has Figure 1 characteristics.

[0087] The following Test Examples 1-7 and Comparative Test Examples 1-2 illustrate the anthraquinone degradation product regeneration method.

[0088] Test Example 1-7

[0089] Test Examples 1-7 illustrate the effect of using the catalysts prepared in Examples 1-7 to carry out anthraquinone degradation product regeneration method reaction in a fixed bed reactor.

[0090] A mixed solution of heavy aromatic hydrocarbons containing amyl anthraquinone and diisobutyl carbinol (DIBC) was used as the working solution, including 170.0 g / L amyl anthraquinone, 37.4 g / L tetrahydro amyl anthraquinone, 4.5 g / L tetrahydro anthraquinone epoxide, 5.2 g / L hydroxyanthraquinone, and 3.2 g / L anthraquinone. 20 g of catalyst was weighed and filled into a stainless steel fixed bed with an inner diameter of 10 mm. The working solution was pressurized and metered by a metering pump and then flowed through the catalyst bed from the bottom of the reactor at an air velocity of 1.8 h -1 , reaction temperature 60℃, sample analysis after 6h reaction. HPLC was used to detect the components in the absorption liquid for quantitative analysis, and the results are listed in Table 1.

[0091] Comparative test example 1

[0092] No catalyst was used and the evaluation conditions were the same as in Test Example 1.

[0093] Comparative test example 2

[0094] White clay was used as the catalyst and the evaluation conditions were the same as those in Test Example 1. Figure 2 This is the TPD-CO2 spectrum of the white clay used in comparative test 2.

[0095] Table 1

[0096]

[0097] From the results of the reaction of the anthraquinone degradation product regeneration method with the catalysts prepared in Examples 1-7 in Table 1, it can be seen that the catalyst of the present invention, due to its composite alkaline properties (weak, medium-strong alkaline, strong alkaline position) and high crushing strength, can almost completely convert the degradation products of anthrone compounds, and also has good conversion performance for epoxide-type degradation products, and can convert more tetrahydroanthraquinones into corresponding alkylanthraquinones. Therefore, the anthraquinone degradation product regeneration method of the present invention can greatly increase the total amount of effective anthraquinone and effectively improve the recycling rate of the working solution.

Claims

1. A method for regenerating a circulating working liquid in the production of hydrogen peroxide by anthraquinone process, comprising contacting the circulating working liquid with an anthraquinone degradation product regeneration catalyst to convert anthraquinone-type, hydroxyanthraquinone, tetrahydroanthraquinone epoxide and tetrahydro-2-alkylanthraquinone compounds in the circulating working liquid into anthraquinone-type compounds, characterized in that: The anthraquinone degradation product regeneration catalyst, calculated on a dry basis and based on the weight of the catalyst, comprises 10-98 weight % of aluminum oxide, 1-80 weight % of magnesium oxide, 1-30 weight % of fluoride and 0-10 weight % of an oxide of a transition metal M selected from Group VIB and Group VIIB, wherein the fluoride is one or more of calcium fluoride, magnesium fluoride and aluminum fluoride.

2. The regeneration method according to claim 1, wherein: The anthraquinone degradation product regeneration catalyst comprises 30-92 wt % of aluminum oxide, 2-10 wt % of fluoride, 5-67 wt % of magnesium oxide and 0.2-8 wt % of an oxide of a transition metal M selected from Group VIB and Group VIIB.

3. The regeneration method according to claim 2, wherein: The anthraquinone degradation product regeneration catalyst comprises 48-72 wt % of aluminum oxide, 4-8 wt % of fluoride, 10-40 wt % of magnesium oxide and 1-6 wt % of an oxide of a transition metal M selected from Group VIB and Group VIIB.

4. The regeneration method according to any one of claims 1 to 3, wherein: The oxide of the transition metal M of group VIB is molybdenum oxide or chromium oxide, and the oxide of the transition metal M of group VIIB is manganese oxide.

5. The regeneration method according to claim 1, characterized in that: The TPD-CO2 spectrum of the anthraquinone degradation product regeneration catalyst has three main peaks, which respectively represent the weak alkaline position of the oxide at about 100°C, the medium-strong alkaline position at 306°C, and the strong alkaline position at 660°C.

6. The regeneration method according to claim 1, characterized in that: The anthraquinone degradation product regeneration catalyst is a spherical catalyst with a particle size of 0.5 to 5.0 mm.

7. The regeneration method according to claim 6, characterized in that: The anthraquinone degradation product regeneration catalyst has a strength of 120N / grain to 190N / grain.

8. The regeneration method according to claim 7, characterized in that: The anthraquinone degradation product regeneration catalyst has a strength of 135N / grain to 170N / grain.

9. The regeneration method according to claim 1, characterized in that: The contacting conditions are a temperature of 20-120° C. and a pressure of 0-1.5 MPa, where the pressure is gauge pressure.

10. The regeneration method according to claim 9, characterized in that: The temperature is 30-90°C, and the pressure is 0-1 MPa.

Citation Information

Patent Citations

  • Anthraquinone degradation product regeneration catalyst and preparation method thereof

    CN102728338A

  • Catalyst, preparation method and use thereof, regeneration method of working solution in hydrogen peroxide production by anthraquinone process and production method of hydrogen peroxide

    CN106540685A

  • Method for regenerating working fluid during production of hydrogen peroxide by anthraquinone process

    CN106629620A

  • Process for manufacturing hydrogen peroxide

    US4668499A

  • Alkaline-earth metal fluoride modified alumina supporter, preparation method thereof, and silver catalyst made from alumina supporter and application of silver catalyst in ethylene epoxide (EO) production

    CN102133544A