A TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst and its preparation method and application

By using a TiO2/CuS/MIL-125-NH2 heterojunction photocatalyst with a rough surface polyhedral structure in the photocatalyst, the problems of deactivation and by-product hazards of traditional photocatalysts during the H2S oxidation process are solved, achieving high efficiency, Selective H2S removal and catalyst regeneration.

CN115999642BActive Publication Date: 2024-10-08ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211657158.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-08
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Traditional photocatalysts are prone to deactivation during the H2S oxidation process and the by-product SO2 is harmful, and the degradation efficiency is low. The existing carrier composite catalysts have insufficient selectivity and duration for sulfur, which limits their practical application.

Method used

A TiO2/CuS/MIL-125-NH2 heterojunction photocatalyst with a rough polyhedral structure is used. Through the close contact between the MIL-125-NH2 substrate and TiO2 and CuS nanoparticles, a highly dispersed heterostructure is formed to improve photogeneration. Carrier separation and migration efficiency, and enhanced light absorption capability through Cu ion modification.

Benefits of technology

It significantly improves the visible light utilization rate and H2S degradation efficiency of the photocatalyst, delays the catalyst deactivation time, achieves efficient and selective H2S removal, and maintains the catalyst's recycling capability through deionized water regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115999642B_ABST
    Figure CN115999642B_ABST
Patent Text Reader

Abstract

The present invention relates to a TiO 2 / CuS / MIL‑125‑NH 2 A heterojunction photocatalyst and its preparation method and application belong to the technical field of photocatalysts. 2 / CuS / MIL‑125‑NH 2 Heterojunction photocatalyst, the TiO 2 / CuS / MIL‑125‑NH 2 The heterojunction photocatalyst is a polyhedral structure with a rough surface. 2 The substrate is CuS and TiO 2 The present invention also discloses a TiO 2 / CuS / MIL‑125‑NH 2 A method for preparing a heterojunction photocatalyst, the preparation method comprising: 2 (Ti / Cu) and thioacetamide were dissolved in ethanol and then heat treated to obtain TiO 2 / CuS / MIL‑125‑NH 2 The present invention also discloses a TiO 2 / CuS / MIL‑125‑NH 2 Application of heterojunction photocatalyst in hydrogen sulfide degradation, the application process comprising: 2 / CuS / MIL‑125‑NH 2 Heterojunction photocatalyst is made into photocatalyst film, which can effectively 2 The photocatalytic degradation rate of S can reach 95%. After regeneration with deionized water, the degradation rate of H 2 The adsorption degradation rate of S can still reach 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalysts and relates to a TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst and a preparation method and application thereof. Background Art

[0002] H2S is a representative substance of odorous gases in livestock and poultry farms, with high concentrations and strong biological toxicity. Photocatalytic degradation, as an advanced oxidation technology, has the advantages of stable chemical properties, mild reaction conditions, high efficiency, and low cost, and has great potential for H2S degradation. However, traditional photocatalysts have the following problems: on the one hand, the catalysts are easily deactivated, which may be caused by the deposition of sulfur or sulfate on the catalyst surface to cover the active sites during the photocatalytic oxidation of H2S; on the other hand, by-products mainly composed of SO2 will be formed during the photocatalytic oxidation of H2S. The above problems will lead to a decrease in the degradation efficiency of the photocatalyst and an increase in the hazards of the by-products, which limits its practical application.

[0003] In order to solve the above problems, existing photocatalysts usually combine TiO2 with a carrier with a large specific surface area. Commonly used carriers include SiO2, γ-Al2O3, activated carbon, molecular sieves, etc. Researchers have found that the selectivity and duration of catalysts based on the above carriers for sulfur are still somewhat different from the ideal effect.

[0004] Therefore, as an ideal H2S degradation technology, the reagents used should be inexpensive (non-precious metal doped), green and environmentally friendly, and can achieve H2S removal efficiently and selectively. In addition, the photocatalyst should be able to be regenerated in a simple and low-cost way. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to propose a TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst with a rough surface and a polyhedral structure, which has good adsorption and degradation performance for H2S and SO2.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst. The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is a polyhedral structure with a rough surface, with MIL-125-NH2 as a substrate and CuS and TiO2 nanoparticles on the surface.

[0008] The TiO2 and CuS on the surface of the photocatalyst of the present invention have high dispersion and are in close contact with the MIL-125-NH2 substrate. The large specific surface area of ​​MIL-125-NH2 can effectively alleviate the harm of byproducts to the catalyst and delay the deactivation time of the catalyst. CuS, TiO2 nanoparticles and MIL-125-NH2 form a compact heterostructure, promote the separation and migration of photogenerated carriers, and improve the visible light catalytic efficiency.

[0009] The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention exhibits very strong light absorption capability in the range of 200 to 800 nm. This strong absorption in the entire visible light region can greatly improve the visible light utilization rate of the photocatalyst, increase the generation of electron-hole pairs, and thus enhance the photocatalytic activity.

[0010] Preferably, the particle size of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is 300-600 nm, and the specific surface area is 500-600 m 2 / g.

[0011] More preferably, the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst has a specific surface area loss rate of 15-20% compared to MIL-125-NH2 (Ti / Cu).

[0012] The invention also discloses a method for preparing a TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst. The method comprises: dissolving MIL-125-NH2 (Ti / Cu) and thioacetamide in ethanol, and then performing heat treatment to obtain TiO2 / CuS / MIL-125-NH2.

[0013] Preferably, the mass ratio of the MIL-125-NH2 (Ti / Cu) to thioacetamide is 1:(0.7-1.4).

[0014] More preferably, the solid-liquid mass ratio of the MIL-125-NH2 (Ti / Cu), thioacetamide and ethanol is 1:(30-70).

[0015] Preferably, the heat treatment is carried out at a temperature of 150 to 240° C. and for a time of 1 to 3 hours.

[0016] Preferably, the product after heat treatment is washed, centrifuged and dried to obtain green TiO2 / CuS / MIL-125-NH2.

[0017] Preferably, the preparation method of the MIL-125-NH2(Ti / Cu) comprises:

[0018] S1, dissolving 2-aminoterephthalic acid and tetrabutyl titanate in a mixed solution of N,N-dimethylformamide (DMF) and methanol, stirring evenly, placing in a reaction kettle and heating to obtain MIL-125-NH2(Ti);

[0019] S2. Dissolve MIL-125-NH2 and Cu(NO3)2·3H2O separately and disperse them by ultrasonic. Heat them in an oil bath to obtain Cu ion-modified MIL-125-NH2 (MIL-125-NH2(Ti / Cu)).

[0020] Preferably, the specific surface area of ​​MIL-125-NH2(Ti) is 1000-1200m 2 / g, the specific surface area of ​​MIL-125-NH2(Ti / Cu) is 600~750m 2 / g.

[0021] Compared with the original MIL-125-NH2(Ti)(Ti-MOF), a considerable decrease in surface area and pore volume was observed after Cu ion coordination, proving the coordination of Cu ions with Ti-MOF. And compared with high-temperature pyrolysis, the solvothermal method adopted in the present invention enables TiO2 / CuS / MIL-125-NH2 to retain a higher specific surface area, which not only provides more exposed photocatalytic active sites, but also helps to support the better distribution of photocatalysts in the entire matrix material without obvious agglomeration. In addition, the larger specific surface area can accommodate more H2O molecules, which can easily interact with the catalytic active sites in the composite material, thereby improving the photocatalytic activity.

[0022] Preferably, the mass ratio of 2-aminoterephthalic acid to tetrabutyl titanate in step S1 is (5-10):1.

[0023] Preferably, the volume ratio of N,N-dimethylformamide to methanol in step S1 is (5-15):1.

[0024] Preferably, the heating process in step S1 is performed at a temperature of 120 to 155° C. and for a time of 48 to 96 hours.

[0025] More preferably, the heated product is filtered, washed, dried and ground to obtain MIL-125-NH2(Ti) as a yellow powder.

[0026] Preferably, the mass ratio of MIL-125-NH2 and Cu(NO3)2·3H2O in step S2 is (1-5):1.

[0027] More preferably, MIL-125-NH2 and Cu(NO3)2·3H2O are respectively dissolved in a mixed solution of DMF and methanol with the same volume and a mass ratio of 1:(0.8-1.2).

[0028] Preferably, the ultrasonic dispersion time in step S2 is 0.5 to 5 hours.

[0029] Preferably, the oil bath heating temperature in step S2 is 100-140° C. and the heating time is 10-15 h.

[0030] More preferably, the yellow-green crystals are obtained by centrifugation after heating in an oil bath, and then washed with methanol and dried overnight to obtain MIL-125-NH2(Ti / Cu).

[0031] The present invention also discloses an application of a TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst in hydrogen sulfide degradation. The application process comprises preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst into a photocatalyst film, and the photocatalytic degradation rate of H2S can reach 95%; after regeneration by deionized water, the adsorption degradation rate of H2S can still reach 90%.

[0032] Preferably, the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is made into a photocatalyst film, and the photocatalytic adsorption degradation rate of H2S remains stable within 5 hours without the release of intermediate product SO2.

[0033] Further preferably, the method for preparing the photocatalyst film comprises: dissolving the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst in an ethanol solution, dispersing the catalyst and ultrasonicating the solution, and then fixing the catalyst on a 0.1 μm microporous filter membrane by suction filtration.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The TiO2 and CuS nanoparticles generated on the surface of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention make it have a larger specific surface area, thereby obtaining a faster transmission and separation speed of photogenerated carriers, inhibiting the recombination of photogenerated carriers, and improving the photocatalytic efficiency.

[0036] 2. In the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention, TiO2, CuS and MIL-125-NH2 are tightly bound to promote charge separation and transfer and improve the photocatalytic performance of the material.

[0037] 3. The present invention is based on MIL-125-NH2 (Ti / Cu) and adopts an in-situ solvothermal method to retain the large specific surface area of ​​MIL-125-NH2 to the maximum extent, thereby delaying the deactivation of the photocatalyst.

[0038] 4. The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention has a long-term stable adsorption performance for H2S, and the photocatalytic degradation rate of H2S can reach 98.6%. It is also regenerable. After regeneration with deionized water, the degradation rate of H2S can still reach 92.3%. It has good prospects for recycling applications.

[0039] 5. The present invention improves the adsorption performance of TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst for H2S and its intermediate product SO2 by doping with Cu ions, further improves the deep oxidation ability, and reduces the generation of secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a flow chart for the preparation of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst in the present invention.

[0041] Figure 2 These are the TEM images of MIL-125-NH2(Ti)(a), MIL-125-NH2(Ti / Cu)(b) and TiO2 / CuS / MIL-125-NH2(c) in Example 1 of the present invention, and the HETEM images of MIL-125-NH2(Ti)(d) and TiO2 / CuS / MIL-125-NH2(e).

[0042] Figure 3 1 is the BET diagram of MIL-125-NH2(Ti), MIL-125-NH2(Ti / Cu) and TiO2 / CuS / MIL-125-NH2 in Example 1 of the present invention.

[0043] Figure 4 This is the UV-visible diffuse reflectance spectra of MIL-125-NH2(Ti), MIL-125-NH2(Ti / Cu) and TiO2 / CuS / MIL-125-NH2 in Example 1 of the present invention.

[0044] Figure 5 Electrochemical impedance spectra of MIL-125-NH2(Ti), MIL-125-NH2(Ti / Cu) and TiO2 / CuS / MIL-125-NH2 in Example 1 of the present invention.

[0045] Figure 6 This is a diagram of the H2S photocatalytic adsorption degradation device used in the present invention.

[0046] Figure 7 This is a graph showing the H2S adsorption curves of MIL-125-NH2(Ti), MIL-125-NH2(Ti / Cu) and TiO2 / CuS / MIL-125-NH2 in the adsorption stage in Example 1 of the present invention.

[0047] Figure 8 This is the performance diagram of visible light photocatalytic degradation of H2S by MIL-125-NH2 (Ti), MIL-125-NH2 (Ti / Cu) and TiO2 / CuS / MIL-125-NH2 in Example 1 of the present invention.

[0048] Fig. 9 This is the stability and regenerability of the TiO2 / CuS / MIL-125-NH2 photocatalyst in Example 1 of the present invention. DETAILED DESCRIPTION

[0049] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0050] Example 1

[0051] 1. Preparation of TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst:

[0052] (1) MIL-125-NH2(Ti)

[0053] 33.1 mg of 2-aminoterephthalic acid and 4.4 mg of tetrabutyl titanate were weighed separately and dissolved in a mixed solution containing 18 ml of N,N-dimethylformamide (DMF) and 2 ml of methanol solution; the resulting mixture was stirred at room temperature for 30 min using a magnetic stirrer, and then transferred to a reactor with a 100 ml Teflon liner and heated at 150°C for 72 h; after cooling to room temperature, the resulting suspension was filtered by centrifugation and then washed three times with DMF and methanol; the light yellow precipitate was then vacuum dried at 80°C and gently ground with an agate mortar to obtain a yellow powder MIL-125-NH2(Ti), denoted as TM.

[0054] (2) MIL-125-NH2(Ti / Cu)

[0055] 0.5 g of the MIL-125-NH2 prepared above was dispersed in a mixture of DMF and methanol (ratio of 1:1, 25 ml each); and dispersed under ultrasonic treatment for 1 hour; 0.22 g of Cu(NO3)2·3H2O was dissolved in 5 ml of methanol and introduced into the above dispersion, and then placed in an oil bath at 120°C for 12 hours; the yellow-green crystals were collected after centrifugation, and then washed with methanol for solvent exchange; the obtained Cu ion-modified MIL-125-NH2 was dried at 80°C overnight and recorded as TCM.

[0056] (3) TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst

[0057] 100 mg of MIL-125-NH2 (Ti / Cu) and 100 mg of thioacetamide (TAA) were dissolved in 10 ml of ethanol solution respectively, and the above solution was transferred to a stainless steel reactor lined with Teflon and heated at 200°C for 2 h; after cooling to room temperature, it was washed with ethanol and centrifuged at 10000 rpm for 5 min, and finally dried at 60°C overnight to obtain TiO2 / CuS / MIL-125-NH2, recorded as TCM2.

[0058] Figure 1 A flow chart for preparation.

[0059] Figure 2 The TEM images of MIL-125-NH2(Ti)(TM)(a), MIL-125-NH2(Ti / Cu)(TCM)(b) and TiO2 / CuS / MIL-125-NH2(TCM2)(c), and the HETEM images of TM(d) and TCM2(e). It can be observed that TM(a)(d) presents a regular polyhedral structure with a particle size of 300-600nm; TCM(b) coordinated by Cu ions does not have any agglomeration and the polyhedral structure is not deformed, which indicates that MIL-125-NH2(Ti) is highly stable to post-synthetic coordination; the polyhedral structure of TCM2(c) is corroded, CuS and TiO2 nanoparticles are generated on its surface, and there is no interlayer gap between TiO2, CuS and MIL-125-NH2. The spacing between the lattice fringes in (e) is 0.193nm and 0.273nm, corresponding to the (110) and (103) planes of the hexagonal CuS respectively, and the spacing between the lattice fringes is 0.352nm, corresponding to the (101) plane of the rutile TiO2. The above results indicate that a heterojunction is formed between the two materials.

[0060] Figure 3The BET diagrams of TM, TCM and TCM2 are shown in Figure 1. As can be seen from the figure, at 77K, due to the capillary filling effect of the micropores, the N2 adsorption-desorption isotherm of TM is consistent with type I. TM has high adsorption performance when the relative pressure (P / P0) is lower than 0.1. Its adsorption and desorption isotherms are reversible and there is no obvious hysteresis loop, indicating that there is a uniform microporous structure in the material. The specific surface area of ​​TM is 1099.15m 2 Compared with the original TM, a considerable decrease in the surface area and pore volume of TCM was observed after the coordination of Cu ions, and its specific surface area decreased to 641.84 m 2 / g, proving that Cu ions are clearly coordinated with TM. TCM2 shows a small hysteresis loop above a relative pressure of 0.4, with no significant loss in its porous properties and a smaller loss in specific surface area compared to its precursor TCM, specifically 527.78 m 2 / g.

[0061] Figure 4 The UV-visible diffuse reflectance spectra of TM, TCM and TCM2 are shown in Figure 2. MIL-125-NH2 (TM) shows a major absorption peak at 400nm, which is caused by the n-π* conversion of the -NH2 functional group. However, when Cu ions are coordinated with TM, the intensity of n-π* conversion is significantly reduced, which further indicates that Cu ions are successfully coordinated through the -NH2 group of TM. It is worth noting that the dd conversion causes the absorption edge of the photocatalyst to red-shift from 475nm to 506nm, and Cu ion coordination can greatly improve the absorption of the visible light region caused by dd conversion, which is consistent with the color change of MOF (after Cu ion coordination, the color changes from bright yellow to yellow-green). At the same time, Cu ion coordination shows a broad absorption peak at 700nm, which is due to the surface plasmon resonance (SPR) effect. Under the action of CuS, the absorption band edge of TCM2 moves to a higher wavelength and shows very strong light absorption ability in the entire measurement wavelength range (200-800nm). This strong absorption in the entire visible light region can greatly improve the visible light utilization of photocatalysts, increase the generation of electron-hole pairs, and thus enhance the photocatalytic activity.

[0062] Figure 5 Figure 2 is the electrochemical impedance spectra of TM, TCM, and TCM2. TCM2 exhibits a smaller semicircle in the electrochemical impedance spectrum than the original TM, indicating that the heterostructure has a lower charge transfer resistance, thus allowing for the rapid transport of photogenerated charges.

[0063] 2. Application:

[0064] The MIL-125-NH2(Ti), MIL-125-NH2(Ti / Cu), and TiO2 / CuS / MIL-125-NH2 prepared as described above were respectively made into photocatalyst films.

[0065] The specific preparation process includes: dissolving 15 mg of the photocatalyst in anhydrous methanol, and fully dispersing it by ultrasonic treatment for 15 minutes, then evenly loading it on a PTFE microporous filter membrane (47 mm, 0.22 μm) by suction filtration, and vacuum drying the filter membrane at 80°C for use.

[0066] The prepared photocatalyst film is placed in a photocatalytic reactor.

[0067] Figure 6 Figure 2 is a diagram of the entire H2S photocatalytic degradation device used.

[0068] The preparation steps for the H2S photocatalytic adsorption degradation experiment include:

[0069] Before the test, the photocatalyst film was pretreated in a vacuum drying oven at 150°C overnight to remove any moisture or residue. After cooling to room temperature, the photocatalyst film material was placed on the supporting net inside the reactor. The reaction system was placed in darkness. The adsorption performance of the prepared material was evaluated at a concentration of 50ppmv and a flow rate of 300ml / min at 1bar. After reaching adsorption saturation, the light source was turned on to carry out the H2S photocatalytic degradation test under visible light.

[0070] A blank test was set up to confirm that the PTFE microporous filter membrane did not adsorb and photocatalytically oxidize H2S under the set test conditions.

[0071] The specific steps of the H2S photocatalytic degradation test include:

[0072] Gaseous H2S was provided by a standard H2S cylinder (1000ppmv); high-purity air was divided into two paths, one was provided with water vapor through a deionized water stripping bottle, and the other was adjusted for humidity through a rotor flowmeter; finally, all branches were evenly mixed in a mixing bottle and entered the reactor at a flow rate of 300ml / min; the light intensity was 50mW·cm -2 A 400W long arc xenon lamp with a UV cut-off filter was used as the visible light source. The concentrations of H2S and SO2 were measured by a multi-gas detector. During the reaction, the photocatalytic reactor was cooled by two fans to maintain the reaction at room temperature.

[0073] Figure 7The H2S adsorption curves of TM, TCM and TCM2 in the adsorption stage. In the breakthrough curve (25°C), the horizontal axis represents the time required for breakthrough (min) and the vertical axis represents the H2S concentration at the outlet (ppmv). The H2S breakthrough capacity of the photocatalyst is determined when the outlet H2S concentration reaches 10% of the inlet concentration. To ensure the reliability of the test data, the breakthrough curve and adsorption capacity of each sample are the average results of 3 tests.

[0074] from Figure 7 It can be seen that the dark adsorption properties of the three are as follows: MIL-125-NH2(Ti) reached adsorption saturation in less than 5 minutes, indicating that it has no obvious adsorption capacity; MIL-125-NH2(Ti / Cu) exhibited a H2S adsorption performance of 1.29mmol / g. Compared with MIL-125-NH2(Ti), the adsorption amount of MIL-125-NH2(Ti / Cu) modified with Cu ions showed a significant increase, which was due to the strong adsorption effect of Cu ions on H2S; TiO2 / CuS / MIL-125-NH2 showed a higher adsorption capacity, reaching 2.05mmol / g. The increase in adsorption capacity was attributed to the increase in the proportion of Cu ions caused by solvent thermal treatment.

[0075] Figure 8 The performance diagram of H2S degradation by visible light photocatalytic adsorption of TM, TCM and TCM2. It can be seen that the TCM2 composite material has a higher H2S photocatalytic degradation rate, and the H2S degradation rate remains basically stable within the reaction time of 5 hours after turning on the light, which can reach more than 98%, and the release of the intermediate product SO2 is not detected during this period (turn off the light source after 5.5 hours and stop the test). Through the above analysis, it can be found that the composite material system that combines adsorption characteristics with photocatalytic characteristics has excellent comprehensive properties. On the one hand, the composite material can promote the removal of H2S on the surface of the material and leave adsorption points for new H2S molecules; on the other hand, the composite material can further oxidize the by-product SO2, thereby effectively preventing secondary pollution.

[0076] Fig. 9 Figure 2 shows the stability and renewability of TCM2 photocatalyst. During the photocatalytic degradation of H2S, the byproduct SO4 2-The deposition of H2S caused the degradation rate of H2S to decrease continuously. After 72 hours of continuous reaction, the degradation rate dropped from 99.8% to 22.4% (the right figure is a bar graph of the degradation rate at 1 hour, 5 hours, 72 hours, and 1 hour after washing). When trying to regenerate the photocatalyst by washing with deionized water, it can be found that the degradation rate can reach up to 92.3%, which is slightly lower than that of the fresh photocatalyst. This may be due to the loss of catalyst during the continuous washing and drying process; the pH value of the deionized water after rinsing is reduced, and ion chromatography analysis confirms the presence of sulfate species on the catalyst surface. The results show that treating the photocatalyst with deionized water can reduce the acidity of the catalyst surface and remove the sulfate accumulated on the catalyst surface, maintaining the catalyst activity in an economical and environmentally friendly way, providing a solution for catalyst regeneration.

[0077] The specific performance of TCM2 is shown in Table 1.

[0078] Example 2

[0079] Compared with Example 1, the difference is that the mass ratio of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) is 1:0.8.

[0080] Example 3

[0081] Compared with Example 1, the difference is that the mass ratio of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) is 1:1.2.

[0082] Example 4

[0083] Compared with Example 1, the difference is that the mass ratio of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) is 1:1.5.

[0084] Example 5

[0085] Compared with Example 1, the difference is that the mass ratio of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) is 1:0.6.

[0086] Example 6

[0087] Compared with Example 1, the difference is that the heat treatment temperature of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 180°C.

[0088] Example 7

[0089] Compared with Example 1, the difference is that the heat treatment temperature of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 230°C.

[0090] Example 8

[0091] Compared with Example 1, the difference is that the heat treatment temperature of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 140°C.

[0092] Example 9

[0093] Compared with Example 1, the difference is that the heat treatment temperature of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 250°C.

[0094] Example 10

[0095] Compared with Example 1, the difference is that the heat treatment time of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 1.5 h.

[0096] Embodiment 11

[0097] Compared with Example 1, the difference is that the heat treatment time of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 2.5 h.

[0098] Example 12

[0099] Compared with Example 1, the difference is that the heat treatment time of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 0.5 h.

[0100] Embodiment 13

[0101] Compared with Example 1, the difference is that the heat treatment time of MIL-125-NH2 (Ti / Cu) and thioacetamide (TAA) in the reactor is 3.5 h.

[0102] Comparative Example 1

[0103] Compared with Example 1, the difference is that the prepared MIL-125-NH2(Ti) is directly reacted with TAA, and other conditions are the same.

[0104] Comparative Example 2

[0105] Compared with Example 1, the difference is that MIL-125-NH2 (Ti / Cu) prepared in CN114471727A is used to react with TAA, and other conditions are the same.

[0106] The specific performance is shown in Table 1.

[0107] Table 1. Performance data of photocatalyst

[0108]

[0109] As can be seen from Table 1, the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst constructed in situ by the solvothermal method of the present invention has an excellent adsorption degradation rate of H2S, which can be as high as 98.6%; and the photocatalyst is regenerable, and after regeneration with deionized water, the adsorption degradation rate of H2S still reaches 92.3%. And within the scope of the present invention, the adsorption degradation rate of H2S by the photocatalyst is higher than 95%, and after regeneration with deionized water, the adsorption degradation rate of H2S can reach 90%.

[0110] In Example 2, due to the decrease in the proportion of TAA, the amount of MIL-125-NH2 converted into TiO2 is reduced, and the amount of CuS also decreases. Therefore, in the early stage of degradation, the degradation rate of Example 2 is slightly lower than that of Example 3. However, because the larger specific surface area of ​​Example 2 delays the deactivation of the material, the degradation rate is slightly better after 72 hours.

[0111] In Comparative Example 1, the prepared MIL-125-NH2(Ti) is directly reacted with TAA, resulting in a significant decrease in the adsorption amount and visible light catalytic performance. This is because MIL-125-NH2(Ti) directly reacts with TAA to generate TiO2. Due to the lack of adsorption of Cu ions and the small specific surface area of ​​TiO2, its adsorption performance for H2S is greatly reduced. At the same time, due to the weak visible light reaction ability of TiO2, its visible light catalytic performance is poor. In Comparative Example 2, the MIL-125-NH2(Ti / Cu) prepared in CN114471727A is reacted with TAA, resulting in a decrease in the adsorption amount and visible light catalytic performance. This is because the Cu ion content in the MIL-125-NH2(Ti / Cu) prepared by this method is limited and unevenly distributed.

[0112] In summary, the TiO2 and CuS nanoparticles generated on the surface of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention make it have a larger specific surface area, thereby obtaining a faster photogenerated carrier transmission and separation speed, inhibiting the recombination of photogenerated carriers, and improving the photocatalytic efficiency; and the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst of the present invention has a long-term stable adsorption performance for H2S, and the photocatalytic degradation rate of H2S can reach 99.8%; and it is regenerable, and after regeneration with deionized water, the degradation rate of H2S still reaches 92.3%; it has good prospects for circular application; the present invention improves the adsorption performance of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst for H2S and its intermediate product SO2 by doping with Cu ions, further improves the deep oxidation ability, and reduces the generation of secondary pollution.

[0113] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst, characterized in that: The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is a polyhedral structure with a rough surface, with MIL-125-NH2 (Ti) as the substrate and CuS and TiO2 nanoparticles on the surface; The preparation method of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst comprises: S1, dissolving 2-aminoterephthalic acid and tetrabutyl titanate in a mixed solution of N,N-dimethylformamide and methanol, stirring evenly, placing in a reaction kettle and heating to obtain MIL-125-NH2(Ti); S2, dissolving MIL-125-NH2(Ti) and Cu(NO3)2•3H2O respectively, dispersing by ultrasonic, and heating in an oil bath to obtain MIL-125-NH2(Ti / Cu); S3. Dissolve MIL-125-NH2 (Ti / Cu) and thioacetamide in ethanol at a mass ratio of 1: (0.7-1.4), and obtain TiO2 / CuS / MIL-125-NH2 by heat treatment; the heat treatment temperature is 150-240°C, and the time is 1-3h.

2. The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 1, characterized in that: The particle size of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is 300-600 nm, and the specific surface area is 500-600 m 2 / g.

3. The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 1, characterized in that: The specific surface area of ​​MIL-125-NH2(Ti) is 1000~1200m 2 / g, the specific surface area of ​​MIL-125-NH2 (Ti / Cu) is 600~750m 2 / g.

4. The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 1, characterized in that: Compared with MIL-125-NH2 (Ti / Cu), the specific surface area loss rate of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is 15-20%.

5. A method for preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst as claimed in claim 1, characterized in that: The preparation method comprises: S1, dissolving 2-aminoterephthalic acid and tetrabutyl titanate in a mixed solution of N,N-dimethylformamide and methanol, stirring evenly, placing in a reaction kettle and heating to obtain MIL-125-NH2(Ti); S2, dissolving MIL-125-NH2(Ti) and Cu(NO3)2•3H2O respectively, dispersing by ultrasonic, and heating in an oil bath to obtain MIL-125-NH2(Ti / Cu); S3. Dissolve MIL-125-NH2 (Ti / Cu) and thioacetamide in ethanol at a mass ratio of 1: (0.7-1.4), and obtain TiO2 / CuS / MIL-125-NH2 by heat treatment; the heat treatment temperature is 150-240°C, and the time is 1-3h.

6. The method for preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 5, characterized in that: The heating process temperature in step S1 is 120-155° C. and the heating time is 48-96 hours.

7. The method for preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 5, characterized in that: The oil bath heating temperature in step S2 is 100-130° C. and the heating time is 10-15 h.

8. The method for preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 5, characterized in that: The mass ratio of the MIL-125-NH2 (Ti / Cu) and thioacetamide is 1: (0.8-1.2).

9. The method for preparing the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst according to claim 5, characterized in that: The heat treatment temperature is 180-230° C. and the time is 1.5-2.5 hours.

10. Use of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst as claimed in claim 1 in hydrogen sulfide degradation, characterized in that: The application process includes preparing a TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst into a photocatalyst film, and the photocatalytic degradation rate of H2S can reach 95%; After regeneration with deionized water, the adsorption and degradation rate of H2S can still reach 90%; The preparation method of the photocatalyst film comprises: dissolving TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst in an ethanol solution, dispersing and ultrasonicating the solution, and then fixing the solution on a 0.1 μm microporous filter membrane by suction filtration.

11. The use of the TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst in hydrogen sulfide degradation according to claim 10, characterized in that: The TiO2 / CuS / MIL-125-NH2 heterojunction photocatalyst is used to make a photocatalyst film, and the photocatalytic adsorption degradation rate of H2S remains stable within 5 hours without releasing the intermediate product SO2.