A combined pretreatment method and system for waste plastics
Through the combined pretreatment method of waste plastic, including extrusion dehydration and dechlorination and deimpurity treatment, the Cl and Si impurities content in the pyrolytic oil is reduced, and the high impurities of harmful elements in the pyrolytic oil in the waste plastic in the prior art are solved. Problem, improving processing efficiency and environmental protection.
Patent Information
- Application Number
- CN202111234535.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-22
AI Technical Summary
In the prior art, the content of harmful elements Cl and Si in waste plastic pyrolyzed oil is high, resulting in the problems of easy corrosion of pipelines and equipment in subsequent process processes and easy deactivation of catalysts.
The combined pretreatment method of waste plastics is adopted, including the extrusion dehydration and dechlorination unit of waste plastics and the deimpurity treatment unit. Through the action of pretreatment agent and solvent oil, the content of chlorine and silicon impurities is reduced, forming a demissible plastic-containing solution, and through The extraction and recycling unit is further processed to reduce pollution and resource consumption in subsequent processing.
It effectively reduces the content of chlorine and silicon impurities in waste plastics, avoids corrosion of subsequent processing units and catalyst deactivation problems, improves processing efficiency, reduces pollution and resource consumption, and has good environmental and economic benefits.
Smart Images

Figure CN116000047B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste plastic treatment, and in particular to a combined pretreatment method and system for waste plastics. Background Art
[0002] The development of the plastics industry has made a huge contribution to social development. At present, my country's annual plastic production has reached about 120 million tons, most of which are discarded into the environment after one use. According to statistics, my country's waste plastic production is about 2.4 to 4.8 million tons per year; by 2035, there will be about 8 billion tons of waste plastic in the natural environment. Since it takes 200 to 500 years for plastic to be completely degraded, the continuous accumulation of waste plastics has not only caused serious environmental pollution, but also affected the ecological balance in the natural environment.
[0003] The existing waste plastic treatment technologies mainly include landfill and incineration. In addition to occupying a large amount of land, landfill is very likely to cause secondary pollution and cannot fundamentally solve the problem. At present, there are only about 400 waste incineration power plants in China that can handle waste plastics. If all waste plastics are to be treated by waste incineration power generation, it is estimated that more than 1,000 plants will still need to be built, which is obviously not feasible. In addition, the physical recycling process of waste plastics is costly, has low economic value, and companies are not profitable enough. In addition, the recycling process is prone to secondary pollution, all of which have led to the slow development of waste plastic resource recycling.
[0004] Chemical conversion of waste plastics is an effective means to achieve rapid recycling and conversion of waste plastics, especially thermoplastic waste plastics can be obtained through pyrolysis process to obtain oil and gas. Therefore, pyrolysis process is currently one of the main process routes for chemical conversion of waste plastics.
[0005] CN106635115B discloses a method and a hydrothermal reaction system for efficiently and cleanly producing oil from mixed waste plastics, the method comprising using an alkaline aqueous solution to perform thermal hydrolysis treatment on the mixed waste plastics at a temperature of 160 to 300°C and a pressure of 20 to 220 bar; the mixed waste plastics contain one or more of polyethylene (PE), polypropylene (PP), polystyrene (PS), and PET, and the mixed waste plastics may also include polyvinyl chloride (PVC); the aqueous phase and the solid phase in the hydrothermally treated material are separated, and the separated solid phase is used to produce oil. The present application not only avoids the adverse effects of PET and PVC in the mixed waste plastics on the oil quality, can produce oil efficiently and cleanly, but also can produce high value-added products, such as TA powder or granules, PS recycled plastics.
[0006] CN108456328A discloses a method for treating waste plastics, comprising: adding waste plastics, a modified catalyst, and a reaction solvent into a catalytic cracking reactor and mixing them evenly, and then performing a catalytic cracking reaction, characterized in that: the modified catalyst is a HZSM-5 and HY composite molecular sieve catalyst modified by a modifier oxide, the modifier is selected from one or more of Sn, Fe, Ti and Zn, the reaction solvent is a mixture of tetralin and n-hexadecane, and the catalytic cracking reaction conditions are as follows: the reaction temperature is 150-300°C, the reaction time is 120-240 minutes, the reaction is carried out under stirring, the stirring rate is 600-1000 rpm, hydrogen is introduced into the reaction, and the hydrogen partial pressure is 4-7MPa.
[0007] Due to the complex composition of waste plastics, which contain a large number of heteroatoms; a large number of organic or inorganic additives are added during the production of plastics to improve the performance of plastics; plastics are prone to adhere to a large number of impurities during the discard process, etc., the main problem of the pyrolysis process in the prior art is that the quality of the pyrolysis oil does not meet the standards, especially the high content of Cl and Si impurities. The Cl in the pyrolysis oil mainly comes from the decomposition of PVC in the waste plastics, mostly small molecular organic chlorine, which is easy to decompose to form HCl in the subsequent oil processing process and cause serious corrosion. In the prior art, the dechlorination of pyrolysis oil mainly adopts hydrogenation to convert organic chlorine into HCl and then neutralize it with alkaline substances, but this produces a large amount of solid waste on the one hand, consumes a large amount of hydrogen resources and increases the cost of catalysts on the other hand. The Si in the pyrolysis oil mainly comes from the decomposition of polymer additives such as silicone oil, silicone resin, silicone rubber powder, and inorganic additives such as SiO2, mainly alkyl epoxy silane, which is a poison for the catalyst of the subsequent processing process and will cause permanent deactivation of the catalyst.
[0008] Therefore, there is still an urgent need for a new waste plastic treatment technology to solve the problem in the prior art that the harmful elements Cl and Si impurities in the waste plastic pyrolysis oil are high, which makes the subsequent process pipelines and equipment prone to corrosion and the catalyst prone to deactivation. Summary of the invention
[0009] The present invention aims to solve the problem in the prior art that the harmful elements Cl and Si impurities in the pyrolysis oil of waste plastics are high, which leads to easy corrosion of pipelines and equipment in the subsequent process and easy deactivation of catalysts, thereby providing a combined pretreatment method and system for waste plastics.
[0010] A first aspect of the present invention provides a combined pretreatment method for waste plastics, comprising the following steps:
[0011] (1) Waste plastic extrusion dehydration and dechlorination unit. The waste plastic enters the waste plastic extrusion dehydration and dechlorination unit, is first dehydrated at temperature T1, and then dechlorinated at temperature T2. The temperature T2 is 50 to 360°C higher than the temperature T1, to obtain dechlorinated waste plastic.
[0012] (2) The dechlorinated waste plastic obtained in step (1) enters a waste plastic impurity removal treatment unit, contacts with a pretreatment agent and solvent oil for impurity removal treatment, and the obtained effluent is subjected to solid-liquid separation to obtain insoluble matter and a de-impurified plastic-containing solution, wherein the metal content of the de-impurified plastic-containing solution is less than 5 μg / g, the chlorine content is less than 20 μg / g, and the silicon content is less than 3 μg / g; the pretreatment agent is selected from one or more of humus, red mud, waste catalyst of an oil refinery, kaolin, semi-coke, activated carbon, gasification ash, and optional alkaline oxides.
[0013] In the present invention, the waste plastic is one or more of the waste plastics in fresh domestic waste, waste plastics in industrial and agricultural production, and waste plastics in aged waste. It can be one or more of the waste plastic rods, waste plastic particles, waste plastic sheets, etc. formed by the preliminary processing of the above-mentioned waste plastics. Preferably, it is waste plastics of poor quality that cannot be physically recycled and regenerated, and the types of waste plastics are one or more of PE, PP, PS, and PVC.
[0014] In one embodiment of the present invention, the waste plastics are roughly crushed before entering the waste plastic extrusion dehydration and dechlorination unit, and the particle size of the crushed waste plastics is 1 to 200 mm, preferably 1 to 50 mm. In one embodiment of the present invention, the waste plastics are washed and dried before crushing.
[0015] In one embodiment of the present invention, in the waste plastic extrusion dehydration and dechlorination unit, the waste plastic is first squeezed out of water at a temperature T1 under pressure, and then further heated to a temperature T2, so that the PVC is decomposed and chlorine-containing compounds such as HCl are discharged to obtain dechlorinated waste plastic.
[0016] In one embodiment of the present invention, in the waste plastic extrusion dehydration and dechlorination unit, the temperature range of T1 is 0-50° C., the temperature range of T2 is 100-350° C., and the extrusion pressure range is 5-30 MPa.
[0017] In a preferred case, the temperature range of T1 is 0-20°C, the temperature range of T2 is 200-300°C, and the pressure range of extrusion is 10-20 MPa.
[0018] In one embodiment of the present invention, a screw extruder with an external heat exchange device can be used in the waste plastic extrusion dehydration and dechlorination unit. The external heat exchange device is a two-stage heat exchange device, one of which is a refrigeration and cold preservation device for controlling the temperature of the dehydration process T1, and the other is a heating and heat preservation device for controlling the temperature of the dechlorination process T2. The removed water is mainly discharged in the form of liquid, and the removed chlorine-containing compounds enter the HCl adsorption device and are recovered by contact with the adsorbent. The adsorbent is selected from one or more of water, alkali solution, brine, and solid alkaline substances.
[0019] In one embodiment of the present invention, in step (2), the treatment conditions of the waste plastic impurity removal treatment unit are: temperature of 250-410°C, pressure of 0.1-5 MPa, and residence time of the dechlorinated waste plastic of 10-60 min. In a preferred case, the treatment conditions of the waste plastic impurity removal treatment unit are: temperature of 320-390°C, pressure of 0.5-4.0 MPa, and residence time of the dechlorinated waste plastic of 15-45 min.
[0020] In the present invention, the term "humus soil" refers to a mixture formed by the decay of plant matter and various organic wastes entrained with waste plastics excavated from landfills.
[0021] In the present invention, the term "semi-coke" refers to a solid product generated by pyrolysis of carbon-containing materials such as coal, biomass, and waste plastics at 350-600°C.
[0022] In the present invention, the term "gasification ash" refers to the solid product remaining after carbon-containing materials such as coal, semi-coke, coke, biomass, petroleum coke, waste plastics, etc. react with a gasifying agent at a temperature above 600°C, normal pressure or pressurized conditions.
[0023] In the present invention, the term "red mud" is also called "red mud", which refers to industrial solid waste discharged after extracting alumina from bauxite.
[0024] In the present invention, the term "solvent oil" has a well-known meaning in the art, which is generally a complex mixture of hydrocarbons. Preferably, the "solvent oil" is a distillate oil rich in aromatics, and the distillate oil rich in aromatics can be one of the liquid distillates obtained from petroleum processing, coal pyrolysis, coal direct liquefaction, biomass and / or waste plastic pyrolysis, or a mixture of multiple thereof.
[0025] In one embodiment of the present invention, the distillation range of solvent oil is 80-550° C., the total aromatic content in the solvent oil is higher than 50% by mass, and the content of monocyclic aromatic hydrocarbons is higher than 20% by mass; in a preferred case, the content of monocyclic aromatic hydrocarbons in the solvent oil is higher than 40% by mass. The weight ratio of solvent oil to waste plastics is 1:10-10:1, and in a preferred case, the weight ratio of solvent oil to waste plastics is 1:1-7:1.
[0026] In one embodiment of the present invention, the particle size of the pretreatment agent is in the range of 75 to 150 μm; the weight ratio of the pretreatment agent to the waste plastic is 1:10 to 2:1, preferably 1:7 to 1:5.
[0027] In a preferred embodiment of the present invention, the pretreatment agent is one or more of spent catalytic cracking catalyst, humus, activated carbon, and optionally a basic oxide.
[0028] In the present invention, "optional" means an optional component. In one embodiment of the present invention, the pretreatment agent contains a basic oxide in addition to other components.
[0029] In the waste plastic impurity removal treatment unit, most plastics are dissolved in solvent oil and undergo desiliconization and demetallization reactions under the action of the pretreatment agent. The effluent after impurity removal is subjected to solid-liquid separation to separate insoluble matter and impurity-free plastic-containing solution. In the method of the present application, by using the carefully selected pretreatment agent and solvent oil type, as well as the treatment conditions, the impurity content in the obtained impurity-free plastic-containing solution can be controlled within a desired range, so as to facilitate subsequent further processing and treatment.
[0030] The present invention does not limit the specific method of solid-liquid separation, which can be one or more of various forms of filters and centrifuges. In one embodiment of the present invention, the solid-liquid separation device is provided with a heating and heat preservation device, the heating device is one or more of external heating or internal heating, and the operating temperature of solid-liquid separation is 250-410°C. When the solid-liquid separation device is a filter, the pore size of the filter is 0.1-75 μm, preferably 0.1-10 μm.
[0031] The present invention reduces the chlorine content in waste plastics through the extrusion dehydration and dechlorination process, and effectively avoids the influence of chlorine impurities on subsequent processing units. At the same time, in the waste plastic dechlorination treatment unit of the present invention, metal impurities and silicon impurities in the dechlorinated waste plastics are effectively removed, and the de-impurified plastic-containing solution obtained by the present invention can be used as a hydrocarbon raw material, and continue to be processed in the process of pyrolysis, catalytic cracking and other processes to produce pyrolysis oil, or chemical raw materials such as olefins and aromatics. In one embodiment of the present invention, the metal content in the de-impurified plastic-containing solution is less than 3μg / g, the chlorine content is less than 1μg / g, and the silicon content is less than 1μg / g. The silicon impurities are removed in the original form of the organosilicon polymer added during the plastic processing process, which effectively avoids the influence of silicon impurities on the catalyst of the subsequent processing unit.
[0032] In one embodiment of the present invention, the following steps are also included:
[0033] (3) allowing the insoluble matter obtained in step (2) to enter an extraction unit, contact with an organic solvent for solvent extraction, and subjecting the obtained product to solid-liquid separation to obtain a solid phase material and a liquid phase material, wherein the organic solvent is selected from one or more of benzene, toluene, chloroform, cyclohexanone, ethyl acetate, butyl acetate, carbon disulfide, tetrahydrofuran, and gasoline;
[0034] (4) treating the solid phase material obtained in step (3) in a pretreatment agent recovery unit to obtain a recovered pretreatment agent, and returning part of the recovered pretreatment agent to the waste plastic impurity removal treatment unit in step (2);
[0035] (5) The obtained liquid phase material is subjected to precipitation treatment and separation in a solvent recovery unit to obtain solid plastic particles and recovered organic solvent.
[0036] In one embodiment of the present invention, one or more of a solvent extraction tower or a static mixing extractor is provided in the extraction unit, and the specific operating conditions of the extraction unit are matched with the selected organic solvent. The purpose of the extraction is to remove the solvent oil adhering to the discharged solid phase material, reduce the total amount of discharged solid material, and ultimately achieve the purpose of emission reduction.
[0037] In a preferred embodiment, the organic solvent is selected from one or more of benzene, toluene, chloroform, cyclohexanone, ethyl acetate, butyl acetate, carbon disulfide, tetrahydrofuran, and gasoline.
[0038] In one embodiment of the present invention, the solid phase material obtained from the extraction unit is treated in the pretreatment agent recovery unit, and the treatment is selected from one or more of screening and regeneration treatment methods.
[0039] In one embodiment of the present invention, the liquid phase material obtained in the extraction unit is subjected to precipitation treatment and separation in the solvent recovery unit to obtain solid plastic particles and recovered organic solvent, and the precipitation treatment is selected from one or more of stripping, simple distillation, flash evaporation, and rectification. The specific operating temperature is flexibly adjusted according to the type and ratio of the selected solvent.
[0040] Another aspect of the present invention further provides a system for any of the above methods, comprising a waste plastic extrusion dehydration and dechlorination unit, a waste plastic impurity removal treatment unit, and a solid-liquid separation unit;
[0041] The waste plastic extrusion dehydration and dechlorination unit is provided with a waste plastic inlet, a water outlet, a chlorine-containing compound outlet and a dechlorinated waste plastic outlet;
[0042] The waste plastic impurity removal processing unit is provided with a dechlorinated waste plastic inlet, a pretreatment agent inlet, a solvent oil inlet and a pretreated material outlet; the pretreated material outlet is connected to the inlet of the solid-liquid separation unit; and the solid-liquid separation unit is provided with an insoluble matter outlet and a de-impurity plastic-containing solution outlet.
[0043] In one embodiment of the present invention, the water outlet of the waste plastic extrusion dehydration and dechlorination unit is connected to a condensation device, and further connected to a sewage treatment device.
[0044] In one embodiment of the present invention, the chlorine-containing compound outlet is connected to the HCl adsorption device inlet, and the chlorine-containing compound is contacted with an adsorbent for recovery, and the adsorbent is selected from one or more of water, alkali solution, brine, and solid alkaline substances.
[0045] In one embodiment of the present invention, a screw extruder with an external heat exchange device can be used in the waste plastic extrusion dehydration and dechlorination unit. The external heat exchange device is a two-stage heat exchange device, one stage is a refrigeration and cold preservation device for controlling the temperature of the dehydration process T1, and the other stage is a heating and heat preservation device for controlling the temperature of the dechlorination process T2. The screw extruder can be continuous or intermittent, horizontal or vertical, and can be one or more of no screw, single screw, twin screw, and multi-screw.
[0046] In one embodiment of the present invention, the waste plastic impurity removal processing unit may be a single-stage or multi-stage kettle dissolving device connected in series or in parallel, or a special-shaped dissolving device with a dissolving effect, or a device with the same function such as a continuous spiral extractor. Further preferably, a stirring device and a heating device are provided in the waste plastic impurity removal processing unit. The stirring device may be electrically driven or magnetically driven, and may be one or more of a paddle type, an anchor type, a frame type, and a spiral strip type. The stirring rate of the stirring device may be 1-300r / min, preferably 60-100r / min; the heating device may be one or more of an internal heating type and / or an external heating type. For example, the external heating device may be one or more of a jacket type or a semicircular coil, and the internal heating device may be various types of built-in coils; the heat source may be one or more of electricity, thermal oil, steam, and open flame heating.
[0047] The present invention has no special requirements for the specific form of the solid-liquid separation unit, which can be various forms of filters, centrifuges, or combinations thereof. In a preferred embodiment, the solid-liquid separation unit can be various forms of oil-resistant, organic solvent-resistant continuous automatic solid-liquid separation equipment with insulation function in one or more stages in series, or one or more of various types of filters with automatic filter screen replacement, filter presses with scrapers, cross-flow filters, horizontal screw centrifuges, and screw extrusion desolventizing equipment. Further preferably, the solid-liquid separation unit can be provided with a heating and insulation device, and the heating device can be one or more of external heating or internal heating devices, the external heating device can be one or more of jacketed or semicircular coils, and the internal heating device can be various types of built-in coils; the heat source can be one or more of electricity, thermal oil, steam, and open flame heating. Preferably, the operating temperature of the solid-liquid separation unit can be, for example, 250-410°C. When the solid-liquid separation unit is a filter, the filter screen aperture can be 0.1-75μm, preferably 0.1-10μm.
[0048] In one embodiment of the present invention, the system further comprises an extraction unit, a pretreatment agent recovery unit, and a solvent recovery unit;
[0049] The extraction unit is provided with an insoluble matter inlet, an organic solvent inlet, a solid phase material outlet, and a liquid phase material outlet, and the insoluble matter outlet of the solid-liquid separation unit is connected with the insoluble matter inlet of the extraction unit;
[0050] The pretreatment agent recovery unit is provided with a solid phase material inlet and a pretreatment agent recovery outlet, the solid phase material outlet of the extraction unit is connected to the solid phase material inlet of the pretreatment agent recovery unit, and the pretreatment agent recovery outlet of the pretreatment agent recovery unit is connected to the pretreatment agent inlet of the waste plastic impurity removal treatment unit;
[0051] The solvent recovery unit is provided with a liquid material inlet, a solid plastic particle outlet and a recovered organic solvent outlet, and the liquid material outlet of the extraction unit is communicated with the liquid material inlet of the solvent recovery unit.
[0052] In one embodiment of the present invention, one or more of a solvent extraction tower or a static mixing extractor may be provided in the extraction unit. The specific operating conditions of the extraction unit are matched with the selected second organic solvent. The purpose of the extraction is to remove the solvent oil adhering to the discharged solid phase material, reduce the total amount of discharged solid material, and ultimately achieve the purpose of emission reduction.
[0053] In a preferred embodiment, the solid phase material obtained by the extraction unit is processed in a pretreatment agent recovery unit, and part or all of it is returned to the waste plastic pretreatment unit as a circulating pretreatment agent. The processing method of the pretreatment agent recovery unit can be selected from screening, regeneration, or a combination thereof. The pretreatment agent recovery unit can be in the form of an oscillating screen, a drum screen, a single-stage or multi-stage fluidized bed regeneration furnace, a rotary kiln regeneration furnace, an infrared heating furnace, etc.
[0054] Features of the present invention:
[0055] The present invention provides a combined pretreatment method and system for waste plastics, which first effectively removes chlorine impurities in waste plastics to avoid the influence of chlorine impurities on subsequent processing units; then effectively removes metal impurities and silicon impurities, wherein silicon impurities are removed in the original form of organic silicon polymers added during plastic processing, effectively avoiding the deactivation of related catalysts in subsequent processing processes such as hydrofining, catalytic cracking, catalytic cracking, etc. In addition, the method and system provided by the present invention have small pollution discharge during the production process, good environmental protection, reduced carbon emissions, and good environmental, social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a schematic diagram of one embodiment of the combined pretreatment method for waste plastics provided by the present invention. DETAILED DESCRIPTION
[0057] The present invention will be further described below in conjunction with the accompanying drawings, but the present invention is not limited thereby.
[0058] Figure 1 is a schematic diagram of one embodiment of the combined pretreatment method for waste plastics provided by the present invention, such as Figure 1 As shown, the crushed waste plastic 8 enters the waste plastic extrusion dehydration and dechlorination unit 1, removes water at temperature T1, and the resulting water 10 enters the sewage treatment device, dechlorinates at temperature T2, and the resulting chlorine-containing compound 11 enters the HCl adsorption device 2 to contact with the adsorbent 12 to obtain the recovered chlorine-containing compound 13. The waste plastic is dehydrated and dechlorinated to obtain the dechlorinated waste plastic 9.
[0059] The obtained dechlorinated waste plastic 9 enters the waste plastic impurity removal treatment unit 3, contacts with solvent oil 14 and pretreatment agent 15 for impurity removal treatment, and the obtained effluent 16 is separated into insoluble matter 17 and decontaminated plastic solution 24 through solid-liquid separation unit 4. The obtained insoluble matter 17 enters the extraction unit 5, contacts with organic solvent 18 for solvent extraction, and the obtained product is subjected to solid-liquid separation to obtain solid phase material 21 and liquid phase material 19. After being treated in the pretreatment agent recovery unit 7, at least part of the obtained solid phase material 21 is returned to the waste plastic impurity removal treatment unit 3 as a recovered pretreatment agent 22, and the remaining part of the solid phase material 23 is discharged from the device. The obtained liquid phase material 19 is subjected to precipitation treatment and separation in the solvent recovery unit 6 to obtain solid plastic particles 25 and recovered organic solvent 20, and the recovered organic solvent 20 is recycled.
[0060] The present invention will be further described below in conjunction with embodiments, but the present invention is not limited thereto.
[0061] In the embodiment, the chlorine content in the solid mixture is determined by the coulometric method. The specific method can refer to the standard method of RIPP64-90 (see "Petrochemical Analysis Method" (RIPP Test Method), edited by Yang Cuiding et al., Science Press, published in 1990, pages 164-167, "Measurement of the total chlorine content in crude oil by the coulometric method"). The instrument used is a Thermo Fisher ECS300 microcoulometric analyzer, the sample is a frozen and crushed waste plastic powder sample, and the obtained chlorine content is the total chlorine content of the sample, including organic chlorine and inorganic chlorine.
[0062] In the examples, the chlorine content in the liquid mixture is also measured using the RIPP 64-90 method, except that the sample is a liquid mixture.
[0063] In the embodiment, the silicon content in the liquid mixture is determined by the method of "Determination of additive elements, wear metals and pollutants in used lubricating oils and certain elements in base oils (Inductively coupled plasma emission spectrometry)" (GB17476-1998).
[0064] In the following examples, unless otherwise specified, the waste plastics were crushed using a shearing crusher with a filter screen aperture of 50 mm.
[0065] The waste plastic raw materials used in the embodiments and comparative examples are as follows:
[0066] Waste plastic A is greenhouse film, ground film, etc. in a certain area of Shandong Province, containing some soil and biomass components. After simple cleaning and drying, it is crushed. The ash content of the obtained waste plastic A is 4.3%, and the moisture content is 10.5%. The main plastic components are PE and a small amount of EVA. It also contains trace amounts of other materials such as PP and PS that cannot be separated. The average total chlorine content on a dry basis is about 850μg / g.
[0067] Waste plastic B was sorted from the garbage of a paper mill in Jiangsu Province. After preliminary drying and crushing, the ash content of the obtained waste plastic B was 9.5%, and the moisture content was 15%. The main components of the waste plastic were PE and PP, and it also contained a small amount of PVC, PET, PS, etc. The average total chlorine content on a dry basis was 2.2%.
[0068] Waste plastic C is waste plastic excavated from aged garbage in a landfill in Guangdong. After multi-stage air separation and preliminary drying, it is crushed. The ash content of the obtained waste plastic C is 11.9%, and the moisture content is 12%. The waste plastic is a mixed waste plastic including PE, PP, PS, PET and PVC, and the average total chlorine content on a dry basis is 1.9%.
[0069] Example 1
[0070] The waste plastic extrusion dehydration and dechlorination unit includes a single screw extruder with an external heat exchange device, wherein the external heat exchange device is a two-stage heat exchange device, one stage is a refrigeration and cold preservation device for controlling the temperature of the dehydration process T1, and the other stage is a heating and heat preservation device for controlling the temperature of the dechlorination process T2. The crushed waste plastic A is fed into the single screw extruder, first dehydrated in liquid form at 25°C, then dechlorinated and residual water is removed at 200°C, the removed chlorine-containing compounds enter the HCl adsorption device, contacted with the CaO adsorbent for recovery, and the dechlorinated waste plastic A is obtained from the dechlorinated waste plastic outlet of the single screw extruder, and enters the waste plastic impurity removal treatment unit. The chlorine content in the obtained dechlorinated waste plastic is 79μg / g.
[0071] The waste plastic impurity removal treatment unit adopts an external heating dissolving kettle. After the dechlorinated waste plastic A is mixed with the pretreatment agent and solvent oil, it is subjected to impurity removal treatment at 350°C and 1.5MPa. The residence time of the dechlorinated waste plastic A is 30min. After treatment, the material is separated into insoluble matter and de-impurity plastic-containing solution by the solid-liquid separation unit. The plastic components in the obtained de-impurity plastic-containing solution are mainly PE and PP, with a concentration of 16%, wherein the silicon content is <1μg / g, the chlorine content is 13μg / g, and the total metal content is 3.5μg / g. The insoluble matter is sent to the extraction unit, contacted with tetrahydrofuran for solvent extraction, and the obtained product is separated to obtain solid phase material and liquid phase material. The obtained solid phase material is treated in the pretreatment agent recovery unit, and part of the recovered pretreatment agent is returned to the waste plastic impurity removal treatment unit. The liquid phase material is contacted with the stripping agent water in the solvent recovery unit for stripping treatment. The obtained solid-liquid mixture is filtered to obtain solid plastic particles and a mixed liquid. The obtained mixed liquid is distilled to recover tetrahydrofuran and the stripping agent for recycling.
[0072] The solvent oil used is catalytic cracking light cycle oil, with a distillation range of 180-350° C., a total aromatic content of 69% by mass, and a monocyclic aromatic content of 48% by mass; the weight ratio of the solvent oil to the waste plastic is 5:1.
[0073] The pretreatment agent used is the waste FCC balance agent provided by the refinery, with a particle size of 75 to 150 μm; the weight ratio of the pretreatment agent to the waste plastic is 1:9.
[0074] The stripping agent used is water, the amount used is 3 times of the liquid phase material, and the stripping temperature is room temperature.
[0075] Example 2
[0076] The waste plastic extrusion dehydration and dechlorination unit includes a single screw extruder with an external heat exchange device, wherein the external heat exchange device is a two-stage heat exchange device, one stage is a refrigeration and cold preservation device for controlling the temperature of the dehydration process T1, and the other stage is a heating and heat preservation device for controlling the temperature of the dechlorination process T2. The crushed waste plastic B is fed into the single screw extruder, first dehydrated at 40°C, and then dechlorinated at 400°C. The removed chlorine-containing compounds enter the HCl adsorption device, contact with the CaO adsorbent for recovery, and the dechlorinated waste plastic B is obtained from the dechlorinated waste plastic outlet of the single screw extruder, and enters the waste plastic impurity removal treatment unit. The total chlorine content in the obtained dechlorinated waste plastic is 1.18%, mainly inorganic chlorine.
[0077] The waste plastic pretreatment unit adopts an external heating dissolving kettle. After the dechlorinated waste plastic B is mixed with the pretreatment agent and solvent oil, it is subjected to impurity removal treatment at 300°C and 1.2MPa. The residence time of the dechlorinated waste plastic B is 40min. After treatment, the material is separated into insoluble matter and impurity-free plastic solution by the solid-liquid separation unit. The plastic components in the obtained impurity-free plastic solution are mainly PE and PP, with a concentration of about 14.8%, wherein the silicon content is <1μg / g, the total chlorine content is 12μg / g, and the total metal content is 2.1μg / g. The insoluble matter is sent to the extraction unit, contacted with tetrahydrofuran for solvent extraction, and the obtained product is separated to obtain solid phase material and liquid phase material. The obtained solid phase material is treated in the pretreatment agent recovery unit, and part of the recovered pretreatment agent is returned to the waste plastic impurity removal treatment unit. The liquid phase material is contacted with the stripping agent water in the solvent recovery unit for stripping treatment. The obtained solid-liquid mixture is filtered to obtain solid plastic particles and a mixed liquid. The obtained mixed liquid is distilled to recover tetrahydrofuran and the stripping agent for recycling.
[0078] The solvent oil used is catalytic cracking light cycle oil, with a distillation range of 180-350° C., a total aromatic content of 69% by mass, and a monocyclic aromatic content of 48% by mass; the weight ratio of the solvent oil to the waste plastic is 5:1.
[0079] The pretreatment agent used is humus and CaO, the mass ratio of which is 8:2, and the particle size is 75-150 μm; the weight ratio of the pretreatment agent to the waste plastic is 1:7.
[0080] Example 3
[0081] The treatment device and treatment conditions adopted in the waste plastic extrusion dehydration and dechlorination unit are the same as those in Example 2, and dechlorinated waste plastic B is obtained.
[0082] The waste plastic impurity removal treatment unit adopts an external heating dissolving kettle. After the dechlorinated waste plastic B is mixed with the pretreatment agent and solvent oil, it is treated with impurities at 350°C and 1.8MPa. The residence time of the dechlorinated waste plastic B is 45 minutes. After the reaction, the material is separated into insoluble matter and impurity-free plastic solution by the solid-liquid separation unit. The plastic components in the obtained impurity-free plastic solution are mainly PE and PP, with a concentration of 14.8%, of which the silicon content is less than 3μg / g, the chlorine content is 18μg / g, and the total metal content is 3.8μg / g.
[0083] The solvent oil used is refinery VGO, which has a distillation range of 275-581°C, a total aromatic content of 45.1% by mass, and a monocyclic aromatic content of 21% by mass; the weight ratio of solvent oil to waste plastics is 5:1.
[0084] The pretreatment agent used is activated carbon and Fe2O3, the mass ratio is 9:1, the particle size is 75-150 μm, and the weight ratio of the pretreatment agent to the waste plastic is 1:8.
[0085] Example 4
[0086] The treatment device and treatment conditions adopted in the waste plastic extrusion dehydration and dechlorination unit are the same as those in Example 2, and dechlorinated waste plastic B is obtained.
[0087] The waste plastic impurity removal treatment unit adopts an external heating dissolving kettle. After the dechlorinated waste plastic B is mixed with the pretreatment agent and solvent oil, it is treated with impurities at 350°C and 1.8MPa. The residence time of the dechlorinated waste plastic B is 30 minutes. After the reaction, the material is separated into insoluble matter and impurity-free plastic solution by the solid-liquid separation unit. The plastic components in the obtained impurity-free plastic solution are mainly PE and PP, with a concentration of 14.8%, of which the silicon content is less than 1μg / g, the chlorine content is 11μg / g, and the total metal content is 4.1μg / g.
[0088] The solvent oil used is the catalytic cracking light cycle oil used in Example 2, with a distillation range of 180-350° C., a total aromatic content of 69% by mass, and a monocyclic aromatic content of 48% by mass; the weight ratio of the solvent oil to the waste plastic is 5:1.
[0089] The pretreatment agent used is activated carbon and Fe2O3, the mass ratio is 9:1, the particle size is 75-150 μm, and the weight ratio of the pretreatment agent to the waste plastic is 1:8.
[0090] Comparative Example 1
[0091] The waste plastic raw material, solvent oil, and impurity removal reaction conditions of this comparative example are the same as those of Example 4, except that no pretreatment agent is used in this comparative example. After the reaction, the material is separated into insoluble matter and impurity-free plastic solution by a solid-liquid separation unit. The silicon content of the obtained impurity-free plastic solution is 42 μg / g, the chlorine content is 770 μg / g, and the total metal content is 13 μg / g.
[0092] The impurity content in the decontaminated plastic-containing solution obtained in this comparative example is too high, especially the chlorine content is much higher than that of crude oil, which is easy to cause corrosion to subsequent processing unit equipment and poses a safety hazard.
[0093] Example 5
[0094] The waste plastic extrusion dehydration and dechlorination unit includes a single screw extruder with an external heat exchange device, wherein the external heat exchange device is a two-stage heat exchange device, one of which is a refrigeration and cold preservation / heating and heat preservation device for controlling the temperature of the dehydration process T1, and the other is a heating and heat preservation device for controlling the temperature of the dechlorination process T2. The crushed waste plastic C is fed into the single screw extruder, first dehydrated at 50°C, and then dechlorinated at 300°C. The removed chlorine-containing compounds enter the HCl adsorption device, contact with the CaO adsorbent for recovery, and the dechlorinated waste plastic C is obtained from the dechlorinated waste plastic outlet of the single screw extruder, and enters the waste plastic impurity removal treatment unit. The total chlorine content in the obtained dechlorinated waste plastic is 0.92%, mainly inorganic chlorine.
[0095] The waste plastic pretreatment unit adopts an external heating dissolving kettle. After the dechlorinated waste plastic C is mixed with the pretreatment agent and solvent oil, it is treated with impurities at 350°C and 1.2MPa. The residence time of the dechlorinated waste plastic C is 35 minutes. After treatment, the material is separated into insoluble matter and impurity-free plastic solution by the solid-liquid separation unit. The plastic components in the obtained impurity-free plastic solution are mainly PE and PP, with a concentration of 14.4%, of which the silicon content is 2.3μg / g, the chlorine content is 8.8μg / g, and the total metal content is 1.8μg / g.
[0096] The solvent oil used is catalytic cracking distillate oil with a distillation range of 150-338° C., a total aromatic content of 76.8% by mass, and a monocyclic aromatic content of 63.8% by mass; the weight ratio of the solvent oil to the dechlorinated waste plastic is 5:1.
[0097] The pretreatment agent used is activated carbon and Fe2O3, the mass ratio is 8:2, the particle size is 75-150 μm, and the weight ratio of the pretreatment agent to the waste plastic is 1:8.
[0098] The obtained oil-containing insoluble matter is sent to the extraction unit, contacted with toluene for solvent extraction, and the obtained product is separated to obtain a solid phase material and a liquid phase material. The obtained solid phase material is treated in the pretreatment agent recovery unit, and part of it is returned to the waste plastic pretreatment device as a circulating pretreatment agent. The liquid phase material is subjected to distillation treatment in the solvent recovery unit to obtain a small amount of solid plastic particles (PS) and recovered toluene and a small amount of adhered solvent oil, respectively. It should be noted that the above description is only an arbitrary embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and changes. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A combined pretreatment method for waste plastics, comprising the following steps: (1) Waste plastic extrusion dehydration and dechlorination unit. Waste plastic enters the waste plastic extrusion dehydration and dechlorination unit, is first dehydrated at a temperature T1, and then dechlorinated at a temperature T2. The temperature T2 is 50 to 360° C. higher than the temperature T1, to obtain dechlorinated waste plastic. In the waste plastic extrusion dehydration and dechlorination unit, the temperature T1 ranges from 0 to 50° C., the temperature T2 ranges from 100 to 350° C., and the extrusion working pressure ranges from 5 to 30 MPa. The chlorine-containing compounds removed by the waste plastic extrusion dehydration and dechlorination unit enter the HCl adsorption device and are contacted with an adsorbent for recovery. The adsorbent is selected from one or more of water, alkali solution, brine, and solid alkaline substances. (2) The dechlorinated waste plastic obtained in step (1) enters a waste plastic impurity removal treatment unit, contacts with a pretreatment agent and solvent oil for impurity removal treatment, and the obtained effluent is subjected to solid-liquid separation to obtain insoluble matter and a de-impurified plastic solution, wherein the metal content of the de-impurified plastic solution is less than 5 μg / g, the chlorine content is less than 20 μg / g, and the silicon content is less than 3 μg / g; wherein the distillation range of the solvent oil is 80 to 550° C., the total aromatic content of the solvent oil is higher than 50% by mass, and the monocyclic aromatic content is higher than 20% by mass; the pretreatment agent is selected from one or more of humus, red mud, waste catalyst of an oil refinery, kaolin, semi-coke, activated carbon, gasification ash, and optional alkaline oxides; and the treatment conditions of the waste plastic impurity removal treatment unit are: temperature of 250 to 410° C., pressure of 0.1 to 5 MPa, and residence time of the dechlorinated waste plastic of 10 to 60 min.
2. The method according to claim 1, characterized in that The waste plastics are one or more of waste plastics in fresh domestic waste, waste plastics in industrial and agricultural production, and waste plastics in aged waste. The types of waste plastics are one or more of PE, PP, PS, and PVC.
3. The method according to claim 1, characterized in that The waste plastics are roughly crushed before entering the waste plastic extrusion dehydration and dechlorination unit, and the particle size of the crushed waste plastics is 1 to 200 mm.
4. The method according to claim 1, characterized in that: In the waste plastic extrusion dehydration and dechlorination unit, the temperature range of T1 is 0-20°C, the temperature range of T2 is 200-300°C, and the working pressure range of extrusion is 10-20MPa.
5. The method according to claim 1, characterized in that The treatment conditions of the waste plastic impurity removal treatment unit are: temperature of 320-390°C, pressure of 0.5-4.0MPa, and residence time of the dechlorinated waste plastic of 15-45min.
6. The method according to claim 1, characterized in that The weight ratio of solvent oil to waste plastics is 1:10 to 10:
1.
7. The method according to claim 1, characterized in that The content of monocyclic aromatic hydrocarbons in the solvent oil is higher than 40% by mass; The weight ratio of solvent oil to waste plastics is 1:1 to 7:
1.
8. The method according to claim 1, characterized in that The particle size range of the pretreatment agent is 75 to 150 μm; the weight ratio of the pretreatment agent to the waste plastic is 1:10 to 2:
1.
9. The method according to claim 1, characterized in that: The weight ratio of the pretreatment agent to the waste plastic is 1:7 to 1:
5.
10. The method according to claim 1, characterized in that The pretreatment agent is one or more of spent catalytic cracking catalyst, humus, activated carbon, and optionally alkaline oxide.
11. The method according to claim 1, characterized in that: The operating temperature of the solid-liquid separation in step (2) is 250-410° C.; The dedoped plastic-containing solution has a metal content of less than 3 μg / g, a chlorine content of less than 1 μg / g, and a silicon content of less than 1 μg / g.
12. A method according to any preceding claim, characterised in that The following steps are also included: (3) allowing the insoluble matter obtained in step (2) to enter an extraction unit, contact with an organic solvent for solvent extraction, and subjecting the obtained product to solid-liquid separation to obtain a solid phase material and a liquid phase material, wherein the organic solvent is selected from one or more of benzene, toluene, chloroform, cyclohexanone, ethyl acetate, butyl acetate, carbon disulfide, tetrahydrofuran, and gasoline; (4) treating the solid phase material obtained in step (3) in a pretreatment agent recovery unit to obtain a recovered pretreatment agent, and returning part of the recovered pretreatment agent to the waste plastic impurity removal treatment unit in step (2); (5) The obtained liquid phase material is subjected to precipitation treatment and separation in a solvent recovery unit to obtain solid plastic particles and recovered organic solvent.
13. The method according to claim 12, characterized in that In step (4), the processing of the pretreatment agent recovery unit includes one or more of screening and regeneration processing methods.
14. The method according to claim 12, characterized in that In the solvent recovery unit of step (5), the precipitation treatment is selected from one or more of stripping, simple distillation and rectification.
15. The method according to claim 12, characterized in that In the solvent recovery unit of step (5), the precipitation treatment is carried out by flash evaporation.
16. A system for the method of any one of claims 12 to 15, comprising a waste plastic extrusion dehydration and dechlorination unit, a waste plastic impurity removal treatment unit, and a solid-liquid separation unit; The waste plastic extrusion dehydration and dechlorination unit is provided with a waste plastic inlet, a water outlet, a chlorine-containing compound outlet and a dechlorinated waste plastic outlet. The waste plastic extrusion dehydration and dechlorination unit is a screw extruder with an external heat exchange device. The external heat exchange device is a two-stage heat exchange device, one stage is a refrigeration and cold preservation device for controlling the temperature of the dehydration process T1, and the other stage is a heating and heat preservation device for controlling the temperature of the dechlorination process T2; The waste plastic impurity removal processing unit is provided with a dechlorinated waste plastic inlet, a pretreatment agent inlet, a solvent oil inlet and a pretreated material outlet; the pretreated material outlet is connected to the inlet of the solid-liquid separation unit; and the solid-liquid separation unit is provided with an insoluble matter outlet and a de-impurity plastic-containing solution outlet.
17. The system according to claim 16, characterized in that The system also includes an extraction unit, a pretreatment agent recovery unit, and a solvent recovery unit; The extraction unit is provided with an insoluble matter inlet, an organic solvent inlet, a solid phase material outlet, and a liquid phase material outlet, and the insoluble matter outlet of the solid-liquid separation unit is connected with the insoluble matter inlet of the extraction unit; The pretreatment agent recovery unit is provided with a solid phase material inlet and a recovery pretreatment agent outlet, the solid phase material outlet of the extraction unit is connected with the solid phase material inlet of the pretreatment agent recovery unit, and the recovery pretreatment agent outlet of the pretreatment agent recovery unit is connected with the pretreatment agent inlet of the waste plastic impurity removal treatment unit; The solvent recovery unit is provided with a liquid material inlet, a solid plastic particle outlet and a recovered organic solvent outlet, and the liquid material outlet of the extraction unit is communicated with the liquid material inlet of the solvent recovery unit.