A single crystal silicon polishing alkali etching additive and its application

By using polishing alkali etching additives with specific ratios in single crystal silicon alkali etching, the problem of improving flatness and reflectivity in alkali etching technology is solved, and uniform corrosion and reflectivity of single crystal silicon surface are achieved, ensuring that The quality and strength of the silicon wafer after polishing.

CN116004232BActive Publication Date: 2024-11-15CHANGZHOU JUNHE TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211497699.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-15
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The existing alkali etching technology has shortcomings in improving the flatness and reflectivity of single-crystal silicon solar cell wafers, and it is difficult to control the thinning amount and remove surface pyramid structures and impurities during the polishing process.

Method used

Using a single crystal silicon polishing alkali etching additive, its composition includes vitamin E, sodium iodate, sodium gluconate, malic acid, polyvinylpyrrolidone and sodium carboxymethylcellulose, pH is adjusted through specific ratios and treatment steps. The value and temperature form a stable alkali polishing etching solution for alkali polishing etching of single crystal silicon.

Benefits of technology

It realizes more uniform corrosion on the surface of single crystal silicon, reduces the reaction rate, improves the wettability and reflectivity of the silicon wafer, removes the pyramid structure and impurities on the surface, forms a step structure, controls the thinning amount, and improves polishing. quality of the surface.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of photovoltaic material preparation, and in particular to an additive for single crystal silicon polishing alkali etching. The mass percentage of each component is as follows: vitamin E is 0.8%-1.5%, sodium iodate is 0.4%-2%, sodium gluconate is 1%-3%, malic acid is 0.1%-0.2%, polyvinyl pyrrolidone is 0.01%-0.04%, sodium carboxymethyl cellulose is 0.2%-0.5%, and the balance is water. The invention provides an additive for alkali polishing etching solution. Due to the existence of isotropic corrosion in the alkali polishing corrosion system, the corrosion process will produce the influence of tension, and the influence of tension is a fixed constant. Therefore, adding a surfactant into the reaction system can reduce the surface tension of the interface, reduce the wetting angle, and thus improve the wettability of the silicon wafer. With the addition of the surfactant, the bubbles generated by the corrosion reaction will leave the surface of the silicon wafer more quickly, so that the single crystal silicon surface will produce a corrosion step structure with a more uniform structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic material preparation, and in particular to a single crystal silicon polishing alkali etching additive and application thereof. Background Art

[0002] Faced with the growing global demand for low-carbon, environmentally friendly and clean energy, the need to use solar energy for power generation is becoming more and more urgent. Improving the efficiency of solar cells has become a need of all mankind. The efficiency of monocrystalline silicon solar cells is better than that of polycrystalline silicon solar cells. Currently, more than 99% of photovoltaic solar cells in the international market are monocrystalline silicon solar cells.

[0003] Acid etching can control the etching rate, and the surface morphology of the wafer after etching is good, but the etching rate of acid etching is too fast, resulting in degradation of the flatness of the wafer; compared with acid etching, the etching rate of alkaline etching is low, but alkaline etching can improve the flatness of the wafer, so a wafer with excellent flatness can be obtained. The existing alkaline etching method also has some other defects, such as the surface reflectivity of the silicon wafer, etching and polishing loss, etc., which still need to be improved. With the development of solar cell technology, the requirements for solar cell silicon wafers are getting higher and higher, so it is necessary to improve the existing etching and polishing technology.

[0004] For single crystal silicon, in order to improve the average reflectivity, it is necessary to improve the surface of the single crystal silicon after polishing, which requires that the surface of the single crystal silicon be evenly etched and fully covered with a layer of surface microstructure. Secondly, it is necessary to improve the surface quality of the polished surface, reduce surface cracks, and enhance the bonding ability of screen printing to the polished surface.

[0005] Therefore, we propose a single crystal silicon polishing alkali etching additive and its application to solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a single crystal silicon alkaline polishing etching liquid additive and its application which can reduce the thinning amount of single crystal silicon and make the silicon wafer surface corroded more uniformly.

[0007] The invention discloses a single crystal silicon polishing alkali etching additive, wherein the mass percentage of each component is as follows: vitamin E is 0.8% to 1.5%, sodium iodate is 0.4% to 2%, sodium gluconate is 1% to 3%, malic acid is 0.1% to 0.2%, polyvinyl pyrrolidone is 0.01% to 0.04%, sodium carboxymethyl cellulose is 0.2% to 0.5%, and the balance is water.

[0008] Preferably, the water is industrial distilled water.

[0009] Preferably, the molecular weight of the sodium carboxymethyl cellulose is 400-800.

[0010] Preferably, the preparation method comprises the following steps:

[0011] 0.8% to 1.5% by mass of vitamin E, 0.4% to 2% of sodium iodate, 1% to 3% of sodium gluconate, 0.1% to 0.2% of malic acid, 0.01% to 0.04% of polyvinyl pyrrolidone, and 0.2% to 0.5% of sodium carboxymethyl cellulose are added to the remaining water, and the temperature is controlled to be 105 to 115° C. and refluxed for 18 to 22 hours, and then the mixed solution is adjusted to pH 6 to 8 with potassium hydroxide solution to obtain a single crystal silicon polishing alkali etching additive.

[0012] Preferably, the etching solution for single crystal silicon alkaline polishing comprises the above-mentioned single crystal silicon polishing alkaline etching additive and a base liquid, and the mass ratio of the single crystal silicon polishing alkaline etching additive to the base liquid is (1.2-10):100.

[0013] Preferably, the base liquid is prepared by mixing potassium hydroxide solution and water, the volume ratio of potassium hydroxide solution to water is 4:96, and the concentration of solute in the potassium hydroxide solution is 48wt%.

[0014] Preferably, the method for alkaline polishing and etching of single crystal silicon utilizes the above-mentioned etching solution to perform alkaline polishing and etching on single crystal silicon.

[0015] Preferably, the method comprises the following steps:

[0016] S1. preparing a single crystal silicon polishing alkali etching additive;

[0017] S2, mixing potassium hydroxide solution and water in a volume ratio of 4:96, wherein the concentration of the solute in the potassium hydroxide solution is 48wt%, to obtain a base solution;

[0018] S3, controlling the temperature of the base liquid at 60-65° C., mixing the additive and the base liquid at a mass ratio of (1-10):100 to obtain an etching solution;

[0019] S4. Control the temperature of the etching solution to 60-65°C, put in the silicon wafer after single crystal silicon texturing, and react for 190-220 seconds to obtain a polished and etched silicon wafer.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention provides an alkali polishing etching solution additive. Since there is isotropic corrosion in the alkali polishing etching system, the corrosion process will produce the influence of tension, and the influence of tension is a fixed constant. Therefore, adding a surfactant to the reaction system can reduce the surface tension of the interface and reduce the wetting angle, thereby improving the wettability of the silicon wafer. With the addition of the surfactant, the bubbles generated by the corrosion reaction will leave the surface of the silicon wafer more quickly, thereby producing a more uniform corrosion step structure on the surface of the single crystal silicon.

[0022] 2. After being added into the alkaline etching reaction solution, the additive of the present invention can make the alkaline corrosion reaction more stable and effectively reduce the reaction rate. At the same time, it can control the amount of alkali thinning of the silicon wafer and the reflectivity of the single crystal silicon. It can effectively remove the pyramid structure on the surface of the single crystal silicon after texturing to form a step state, and at the same time, it can remove impurities adsorbed on the surface of the silicon wafer. DETAILED DESCRIPTION

[0023] The present invention will be further explained below in conjunction with specific embodiments.

[0024] The invention discloses a single crystal silicon polishing alkali etching additive, wherein the mass percentage of each component is as follows: vitamin E is 0.8% to 1.5%, sodium iodate is 0.4% to 2%, sodium gluconate is 1% to 3%, malic acid is 0.1% to 0.2%, polyvinyl pyrrolidone is 0.01% to 0.04%, sodium carboxymethyl cellulose is 0.2% to 0.5%, and the balance is water.

[0025] The water is industrial distilled water.

[0026] The molecular weight of the sodium carboxymethyl cellulose is 400-800.

[0027] The method for alkaline polishing and etching of single crystal silicon comprises the following steps:

[0028] S1. Add 0.8% to 1.5% by mass of vitamin E, 0.4% to 2% of sodium iodate, 1% to 3% of sodium gluconate, 0.1% to 0.2% of malic acid, 0.01% to 0.04% of polyvinyl pyrrolidone, and 0.2% to 0.5% of sodium carboxymethyl cellulose to the remaining water, control the temperature to 105 to 115° C. and reflux for 18 to 22 hours, then adjust the mixed solution to pH 6 to 8 with potassium hydroxide solution to obtain a single crystal silicon polishing alkali etching additive;

[0029] S2, mixing potassium hydroxide solution and water in a volume ratio of 4:96, wherein the concentration of the solute in the potassium hydroxide solution is 48wt%, to obtain a base solution;

[0030] S3, controlling the temperature of the base liquid at 60-65° C., mixing the additive and the base liquid at a mass ratio of (1-10):100 to obtain an etching solution;

[0031] S4. Control the temperature of the etching solution to 60-65°C, put in the silicon wafer after single crystal silicon texturing, and react for 190-220 seconds to obtain a polished and etched silicon wafer.

[0032] Examples 1-3 are specific applications of the alkaline polishing and etching additive of the present invention in alkaline polishing and etching of single crystal silicon.

[0033] In Example 1

[0034] 8g vitamin E, 4g sodium iodate, 10g sodium gluconate, 1g malic acid, 0.1g polyvinyl pyrrolidone, 2g sodium carboxymethyl cellulose and 974.9g water were mixed, the temperature was controlled at 110°C, refluxed for 20h, and then the pH was adjusted to 6-8 with potassium hydroxide to obtain a polishing and etching additive;

[0035] Measure 40L of 48% potassium hydroxide and 96L of water, mix and stir evenly to obtain a base solution;

[0036] Weigh 12g of alkaline polishing etching solution and 1000g of base liquid, control the temperature to 60°C, mix evenly, put in the single crystal silicon wafer after texturing, react for 190s, and obtain the polished silicon wafer.

[0037] In Example 2

[0038] Mix 10g vitamin E, 14g sodium iodate, 20g sodium gluconate, 1.3g malic acid, 0.25g polyvinyl pyrrolidone, 3g sodium carboxymethyl cellulose and 951.45g water, control the temperature at 120°C, reflux for 22h, and then adjust the pH to 6-8 with potassium hydroxide to obtain a polishing and etching additive.

[0039] Measure 60L of 48% potassium hydroxide and 150L of water, mix and stir evenly to obtain a base solution;

[0040] Weigh 50g of alkaline polishing etching solution and 1000g of base liquid, control the temperature to 62°C, mix them evenly, put in the single crystal silicon wafer after texturing, react for 200s, and obtain the polished silicon wafer.

[0041] In Example 3

[0042] Mix 15g vitamin E, 20g sodium iodate, 30g sodium gluconate, 2g malic acid, 0.4g polyvinyl pyrrolidone, 5g sodium carboxymethyl cellulose and 927.6g water, control the temperature at 140°C, reflux for 25h, and then adjust the pH to 6-8 with potassium hydroxide to obtain a polishing and etching additive.

[0043] Measure 80L of 48% potassium hydroxide and 180L of water, mix and stir evenly to obtain a base solution;

[0044] Weigh 30g of alkaline polishing etching solution and 1000g of base liquid, control the temperature to 62°C, mix evenly, put in the single crystal silicon wafer after texturing, react for 200s, and obtain the polished silicon wafer.

[0045] Comparative Example 1 is single crystal silicon alkaline polishing and etching without adding alkaline polishing and etching additives.

[0046] Compared with Example 3, Comparative Example 1 does not add polishing and etching additives, and the rest are the same. The specific steps are: measure 80L of 48% mass concentration potassium hydroxide and 180L of water, mix and stir evenly to obtain a base liquid; weigh 1000g of the base liquid, control the temperature to 62°C, mix evenly, put in the single crystal silicon wafer after the texturing is completed, react for 200s, and obtain a polished silicon wafer.

[0047] Examples 1-3 are specific applications of the alkali polishing and etching additives of the present invention in alkali polishing and etching of single crystal silicon, and Comparative Example 1 is alkali polishing and etching of single crystal silicon without adding the alkali polishing and etching additives, and the obtained polishing effects are shown in Table 1;

[0048] Table 1

[0049] Grouping Comparative Example 1 Example 1 Example 2 Example 3 Reflectivity / % 35.46 43.32 43.27 43.30 Open circuit voltage / V 0.6673 0.6809 0.6812 0.6807 Short circuit voltage / V 8.3143 8.5514 8.5532 8.5529 Thinning amount / g 0.51 0.32 0.28 0.30

[0050] In Examples 1-3, the reflectivity is greater than 43.2%, which is significantly better than that of Comparative Example 1, and the thinning amount of Examples 1-3 can be controlled at about 0.3 g, ensuring that the single crystal silicon wafer has a certain strength after alkali polishing and etching.

[0051] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A single crystal silicon polishing alkali etching additive, It is characterized in that The preparation method comprises the following steps: 0.8% to 1.5% by mass of vitamin E, 0.4% to 2% of sodium iodate, 1% to 3% of sodium gluconate, 0.1% to 0.2% of malic acid, 0.01% to 0.04% of polyvinyl pyrrolidone, and 0.2% to 0.5% of sodium carboxymethyl cellulose are added to the remaining amount of water, and the temperature is controlled to be 105 to 115° C. and refluxed for 18 to 22 hours, and then the mixed solution is adjusted to pH 6 to 8 with potassium hydroxide solution to obtain a single crystal silicon polishing alkali etching additive; The molecular weight of the sodium carboxymethyl cellulose is 400-800.

2. The single crystal silicon polishing alkali etching additive according to claim 1, It is characterized in that The water is industrial distilled water.

3. Used for single crystal silicon alkaline polishing and etching liquid, It is characterized in that The etching solution comprises the single crystal silicon polishing alkali etching additive and a base liquid according to any one of claims 1 to 2, wherein the mass ratio of the single crystal silicon polishing alkali etching additive to the base liquid is (1.2 to 10):100; The base liquid is prepared by mixing potassium hydroxide solution and water, the volume ratio of potassium hydroxide solution to water is 4:96, and the concentration of the solute in the potassium hydroxide solution is 48wt%.

4. Method of single crystal silicon alkaline polishing and etching, It is characterized in that The single crystal silicon is alkali-polished and etched using the etching solution described in claim 3.

5. The method for single crystal silicon alkaline polishing and etching according to claim 4, It is characterized in that The following steps are involved: S1. preparing a single crystal silicon polishing alkali etching additive; S2, mixing potassium hydroxide solution and water in a volume ratio of 4:96, wherein the concentration of the solute in the potassium hydroxide solution is 48wt%, to obtain a base solution; S3, controlling the temperature of the base liquid at 60-65° C., mixing the additive and the base liquid at a mass ratio of (1.2-10):100 to obtain an etching solution; S4. Control the temperature of the etching solution to 60-65°C, put in the silicon wafer after single crystal silicon texturing, and react for 190-220 seconds to obtain a polished and etched silicon wafer.