A method for preparing water-based polyurethane microfiber fabric for imitation leather

By controlling the dynamic viscosity of the water-based polyurethane impregnated material and the density of the non-woven fabric, combined with the standing time and heat treatment, the gradient distribution of the polyurethane resin in the ultra-fine fiber synthetic leather is achieved, which solves the problems of complex processes and non-environmental protection in the existing technology. It improves the feel and resilience of the product, while reducing production costs and environmental pollution.

CN116005462BActive Publication Date: 2024-10-01JIANGSU HUAFON MICROFIBRE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211708092.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-10-01
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing ultrafine fiber synthetic leather process is complex and not environmentally friendly, and it is difficult to achieve good gradient distribution of polyurethane resin, resulting in poor feel and high cost.

Method used

By controlling the dynamic viscosity of the water-based polyurethane impregnated material, the density of the non-woven fabric and the liquid-carrying rate, combined with the standing time and heat treatment, the gradient distribution of the polyurethane resin in the non-woven fabric is achieved, and the thermal gelation technology and alkali reduction process are used to achieve Reduce environmental pollution.

Benefits of technology

The process is simplified, the microfiber base cloth has good longitudinal distribution gradient and resilience, and the feel is close to genuine leather, which reduces production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116005462B_ABST
    Figure CN116005462B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a simulated leather water-based polyurethane microfiber base fabric, comprising the following steps: (1) preparing a water-based polyurethane impregnating material; (2) using the water-based polyurethane impregnating material to impregnate a surface-density ρ of 0.23-0.26 g / cm 3 The sea-island fiber nonwoven fabric is prepared by controlling the liquid rate of the water-based polyurethane impregnated material to be 150-240% to obtain a wet cloth; (3) placing the wet cloth horizontally on a platform and letting it stand for t min, t=a×(475ρ-65)±15; (4) controlling the water-based polyurethane impregnated material on the wet cloth after standing to solidify within 1 min; (5) removing the sea phase by reducing the amount after drying to obtain a simulated leather water-based polyurethane microfiber base fabric. The method of the present invention is simple in process, and the polyurethane in the obtained microfiber base fabric has a good longitudinal distribution gradient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ultrafine fiber synthetic leather and relates to a method for preparing a simulated leather waterborne polyurethane ultrafine fiber base cloth. Background Art

[0002] Natural leather has the advantages of being breathable, soft, elastic, and comfortable to wear, and is widely used in life and production; however, natural leather also has disadvantages such as low yield, poor thickness uniformity, shrinkage after washing, and easy to rot. Microfiber synthetic leather is currently considered to be the best material to replace natural leather. It is usually made of sea-island type fibers to make non-woven fabrics and impregnated with polyurethane resin. After fiber opening, each sea-island fiber is separated into a bundle of microfibers to form a three-dimensional interwoven mesh structure. This structure is very similar to the bundled collagen fibers in natural leather. Microfiber synthetic leather even has most physical properties that are better than natural leather. However, in conventional microfiber synthetic leather, the polyurethane resin is evenly distributed from the surface to the inside, and the fiber leather has uniform density from top to bottom. It does not have the gradient structure of natural leather, and the leather feel is poor.

[0003] Prior art CN114086401A discloses a method for preparing a microfiber-based fabric with a good internal structure of polyurethane gradient distribution, which utilizes chemical reaction foaming to promote the movement of polyurethane to achieve the desired polyurethane arrangement and distribution. However, the processing process of this method is too complicated and has too many process control points, which is not conducive to efficient industrial implementation; and the preparation process requires the addition of inorganic acids, etc., which produces certain carbon dioxide emissions.

[0004] Therefore, it is of great significance to study a method for preparing a simulated leather water-based polyurethane microfiber base cloth to solve the problems of complex process and environmental pollution in the prior art. Summary of the invention

[0005] The purpose of the invention is to solve the problems existing in the prior art and provide a method for preparing a simulated leather water-based polyurethane microfiber base cloth.

[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a simulated leather water-based polyurethane microfiber base fabric comprises the following steps:

[0008] (1) preparing waterborne polyurethane impregnated material;

[0009] The dynamic viscosity μ of the waterborne polyurethane impregnation material at a temperature of 25°C is 5-57 mPa·s; the dynamic viscosity of the waterborne polyurethane impregnation material affects the gradient distribution of the final product. When the dynamic viscosity is too large, the sedimentation movement of the waterborne polyurethane impregnation material is difficult;

[0010] (2) Use water-based polyurethane impregnation material with an apparent density of ρ of 0.23-0.26 g / cm 3 The sea-island fiber nonwoven fabric is prepared by controlling the liquid carrying rate of the waterborne polyurethane impregnated material to be 150-240% to obtain a wet fabric;

[0011] Choose 0.23-0.26g / cm 3 The apparent density of the nonwoven fabric is to achieve the purpose of controlling the sedimentation of the waterborne polyurethane in the nonwoven fabric during the impregnation step, the feel of the finished base fabric and the cost. When it is less than 0.23g / cm 3 When the fiber content in the finished base fabric is less, more resin needs to be filled to ensure the hand feel, resulting in higher costs; greater than 0.26g / cm 3 When the fibers in the non-woven fabric are densely arranged, the capillary effect significantly hinders the sedimentation of the waterborne polyurethane in the non-woven fabric, which greatly increases the horizontal settling time or causes no obvious sedimentation.

[0012] The feel of the base fabric is provided by microfibers and polyurethane resin. Since the fiber cost is lower than polyurethane, if the density of non-woven fabric is low, more polyurethane needs to be filled, which leads to a significant increase in cost. If the density is too high, less polyurethane is filled, making the microfiber base fabric lose the comfortable and elastic feel similar to natural leather. Therefore, the existing microfiber technology usually fills the entire internal space of the non-woven fabric with polyurethane resin evenly, and controls the density of the non-woven fabric to 0.275-0.310g / cm 3 , which can reduce costs while providing a good hand feel; however, the existing conventional non-woven fabric density is not suitable for the sedimentation of the waterborne polyurethane in the present invention. The present invention obtains a gradient distribution by controlling the static sedimentation of the waterborne polyurethane after impregnation. Too dense a non-woven fabric density will lead to capillary action, making sedimentation difficult; the present invention controls the density of the non-woven fabric to 0.23-0.26 g / cm 3 , so that the water-based polyurethane is distributed in a gradient in the non-woven fabric, which can not only maintain the elastic and soft feel of the microfiber base fabric, but also give it a differentiated feel similar to that of genuine leather;

[0013] The present invention controls the liquid carrying rate to be 150-240%. If the liquid carrying rate is too high, there will be fewer voids in the non-woven fabric, which is not conducive to the sedimentation of the water-based polyurethane to form a step distribution. If the liquid carrying rate is low, that is, the sizing amount of the water-based polyurethane impregnated material is small, the polyurethane resin has insufficient sedimentation power, and the horizontal placement time is long or no obvious step distribution can be formed.

[0014] (3) Place the wet cloth horizontally on the platform and let it stand for t min, t = a × (475ρ-65) ± 15. Note that the unit of ρ is g / cm 3, when calculating the value of t, only the value of ρ is substituted without the unit; when μ is (1-20]mPa·s, a=0.99; when μ is (21-40]mPa·s, a=1; when μ is (40-60]mPa·s, a=1.01;

[0015] This formula is obtained by statistical experiment results for the non-woven fabric, water-based polyurethane and corresponding auxiliary agent formula mentioned in the present invention. Since the sedimentation of water-based polyurethane emulsion in non-woven fabric is a process that makes polyurethane in non-woven fabric change from uniform distribution → step distribution → bottom concentrated distribution, the experimental results are observed by electron microscope. According to statistics, the water-based polyurethane has a better gradient distribution in the experimental samples within this formula; the horizontal placement time is short, the emulsion sedimentation movement is insufficient, and no obvious gradient distribution appears in the non-woven fabric; the horizontal placement time is too long, the emulsion mainly settles to one side of the bottom surface of the non-woven fabric, and the purpose of gradient distribution of the emulsion in the non-woven fabric is not achieved; the appropriate standing time is positively correlated with the density of the non-woven fabric. The greater the density of the non-woven fabric, the smaller the gap in the non-woven fabric, and the longer the sedimentation time required. a×(475ρ-65) is basically the optimal immersion time, and 15 minutes above or below this time is allowed;

[0016] (4) Control the waterborne polyurethane impregnation material on the wet cloth after standing to solidify within 1 minute; if the solidification time is too long, the waterborne polyurethane impregnated in the non-woven fabric will continue to settle, which will affect the gradient distribution of the waterborne polyurethane in the non-woven fabric;

[0017] (5) After drying, the sea phase is removed by reducing the amount to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0018] The dynamic viscosity of the waterborne polyurethane impregnation material, the density of the non-woven fabric, the liquid carrying rate, the standing time and the curing time are matched to each other, creating a filling state in which the impregnation liquid presents a gradient distribution in the gaps of the non-woven fabric. 3The apparent density of the non-woven fabric is lower than that of the non-woven fabric used in the prior art. This is because the water-based polyurethane used in the present invention has fluidity similar to that of water at room temperature. In the non-woven fabric in this density range, with the increase of horizontal placement time, obvious vertical downward sedimentation will occur, so that the water-based polyurethane is distributed in a gradient in the non-woven fabric. The greater the density of the non-woven fabric, the more obvious the capillary effect, and the weaker the resin sedimentation effect. The liquid carrying rate of the water-based polyurethane impregnation material should be suitable for the apparent density range of the non-woven fabric, and the liquid carrying rate is controlled to be 150-240%. The high liquid carrying rate of the water-based polyurethane impregnation material has few voids in the non-woven fabric, which is not conducive to the penetration of the water-based polyurethane to form a step distribution; the low liquid carrying rate of the water-based polyurethane impregnation material, that is, the amount of water-based polyurethane resin sizing is small, the water-based polyurethane does not have sufficient penetration power, and cannot form an obvious step distribution. In the initial stage of impregnation, the distribution of waterborne polyurethane in the base fabric is relatively uniform. Compared with the traditional process concept, it is necessary to consider the sedimentation capacity of polyurethane, which is determined by the gap between the non-woven fabric and the impregnation liquid rate. After the impregnation, a horizontal placement step is required. In this step, the polyurethane impregnation liquid adjusts its distribution by gravity to obtain a gradient distribution effect. It is left to stand for a specific time. If the time is too short or too long, the gradient distribution will be unsatisfactory. Then, the temperature characteristics of the waterborne polyurethane are used to solidify the gradient distribution in time.

[0019] As the preferred technical solution:

[0020] According to the method for preparing a simulated leather water-based polyurethane microfiber base fabric as described above, in step (1), the water-based polyurethane impregnation material mainly consists of an electrolyte-sensitive water-based polyurethane emulsion and a monovalent electrolyte solution with a mass concentration of 0.7-2.3%, the mass proportion of the monovalent electrolyte solution in the water-based polyurethane impregnation material is ≥15wt%, the solid content of the water-based polyurethane impregnation material and the liquid carrying rate of the water-based polyurethane impregnation material are coordinated to ensure that the water-based polyurethane content in the sea-island fiber non-woven fabric in step (2) is 27%-36%, and the water-based polyurethane content in the sea-island fiber non-woven fabric is % = (solid content of water-based polyurethane impregnation material × liquid carrying rate of water-based polyurethane impregnation material) / (solid content of water-based polyurethane impregnation material × liquid carrying rate of water-based polyurethane impregnation material + 1);

[0021] When the mass proportion of the monovalent electrolyte solution in the waterborne polyurethane impregnating material is greater than 15wt%, the electrolyte solution within this mass concentration range is added to the electrolyte-sensitive waterborne polyurethane emulsion to give the waterborne polyurethane emulsion a thermosensitive property. A low concentration does not have this effect, and a too high concentration will cause the waterborne polyurethane emulsion to demulsify.

[0022] The monovalent electrolyte solution is used as a coagulant. By adjusting the content of the coagulant, the waterborne polyurethane impregnated material can be completely gelled and solidified under the condition of being placed horizontally with a thickness of 2 mm and standing at 80° C. for 1 minute, and loses fluidity. Since the gelling and solidifying behavior of the waterborne polyurethane impregnated material is triggered by temperature, the flow and sedimentation performance of the waterborne polyurethane is not affected at low temperatures. When the temperature rises, the dynamic viscosity of the waterborne polyurethane increases rapidly, the gel is solidified, and the fluidity is lost, and the resin gel is fixed at the corresponding position.

[0023] The content of water-based polyurethane in the sea-island fiber non-woven fabric is low, and the base fabric feels lacking in fleshiness. The content of water-based polyurethane in the sea-island fiber non-woven fabric is high, and the base fabric feels hard and not soft.

[0024] In the method for preparing a simulated leather water-based polyurethane microfiber base fabric as described above, in step (4), curing is carried out by heat treatment, the heat treatment temperature is above 80°C, and the heat treatment time is at least 1 minute. The heat treatment causes the water-based polyurethane impregnated material with a gradient distribution in the non-woven fabric to rapidly increase its dynamic viscosity after being heated, lose its fluidity, and fix the resin gel in the corresponding position, retaining its gradient distribution in the non-woven fabric.

[0025] It should be noted that the purpose of the present invention preferably using thermogel technology (i.e., using an aqueous polyurethane impregnating material containing a monovalent electrolyte and a heat treatment method) is to achieve rapid curing of the aqueous polyurethane impregnating material. The protection scope of the present invention includes but is not limited to this. Other technologies that can achieve rapid curing of aqueous polyurethane impregnating materials are also applicable to the present invention.

[0026] In the method for preparing the simulated leather water-based polyurethane microfiber base fabric as described above, in step (2), the apparent density ρ of the sea-island fiber nonwoven fabric is 0.24-0.245 g / cm 3 .

[0027] In the method for preparing the simulated leather water-based polyurethane microfiber base fabric as described above, in step (2), the sea phase in the sea-island fiber non-woven fabric is a water-soluble polyester.

[0028] In the method for preparing a simulated leather water-based polyurethane microfiber base cloth as described above, in step (5), the reduction is carried out by an alkali reduction or water reduction method; the present invention uses an alkali reduction or water reduction method to extract the sea phase, and no solvent is used in the entire production process to reduce environmental pollution, and the water-reduced sea phase polymer can be reused.

[0029] As described above, the preparation method of the simulated leather water-based polyurethane microfiber base fabric has a rebound time of 50 to 64 seconds. The closer the resin in the simulated leather water-based polyurethane microfiber base fabric is to the ideal gradient distribution, the slower the rebound time. At the same time, the base fabric feels closer to genuine leather and has a soft and differentiated feel of genuine leather.

[0030] Beneficial Effects

[0031] (1) The preparation method of the simulated leather water-based polyurethane microfiber base fabric of the present invention has a simple process;

[0032] (2) The polyurethane in the simulated leather water-based polyurethane microfiber base fabric of the present invention has a good longitudinal distribution gradient;

[0033] (3) The simulated leather water-based polyurethane microfiber base fabric of the present invention has good resilience. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is an electron microscope image of the simulated leather water-based polyurethane microfiber base fabric prepared in Example 1;

[0035] Figure 2 This is an electron microscope image of the waterborne polyurethane microfiber base fabric prepared in Comparative Example 1;

[0036] Figure 3 This is an electron microscope image of the waterborne polyurethane microfiber base fabric prepared in Comparative Example 2;

[0037] Figure 4 This is an electron microscope image of the waterborne polyurethane microfiber base fabric prepared in Comparative Example 3;

[0038] Figure 5 This is an electron microscope image of the waterborne polyurethane microfiber base fabric prepared in Comparative Example 4;

[0039] Figure 6 This is an electron microscope image of the waterborne polyurethane microfiber base fabric prepared in Comparative Example 5. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0041] The testing methods of some indicators in the following embodiments and comparative examples are as follows:

[0042] (1) Polyurethane distribution: Using a scanning electron microscope, the gradient distribution effect of polyurethane was observed in the longitudinal section;

[0043] (2) Rebound time: Prepare a 1 cm × 1 cm × 0.8 mm microfiber synthetic leather base fabric, fold it in half and load it with 1 kg. After keeping it in place for 10 min, remove the pressure, open the microfiber synthetic leather base fabric, and record the time it takes for the fold mark to completely disappear within 10 min. This is the rebound time.

[0044] Example 1

[0045] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0046] (1) preparing waterborne polyurethane impregnated material;

[0047] The waterborne polyurethane impregnation material is prepared by mixing waterborne polyurethane emulsion YS-3000 produced by Dow Chemical (the solid content of polyurethane resin in the emulsion is 54%) and Na2SO4 aqueous solution with a mass concentration of 1.2wt%. During the preparation process, the Na2SO4 aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 24%. The mass proportion of the Na2SO4 aqueous solution in the waterborne polyurethane impregnation material is 55.6%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 5mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0048] (2) The nonwoven fabric is a COPET / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd., with an apparent density of 0.241 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 180%, and obtaining a wet fabric with a polyurethane resin content of 30.2wt%;

[0049] (3) Place the wet cloth horizontally on the platform and let it stand for 49 minutes;

[0050] (4) heat treating the wet cloth at 90° C. for 1 min to complete the curing of the waterborne polyurethane impregnation material;

[0051] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0052] The longitudinal cross-sectional diagram of the finally obtained simulated leather waterborne polyurethane microfiber base fabric is as follows: Figure 1 As shown, the rebound time of the simulated leather water-based polyurethane microfiber base fabric is 64s.

[0053] Comparative Example 1

[0054] A method for preparing a waterborne polyurethane microfiber base fabric is basically the same as in Example 1, except that: the sea-island fiber nonwoven fabric in step (2) is a COPET / PET type island-fixed nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd., and has an apparent density of 0.28 g / cm 3 ; The standing time in step (3) is 67 minutes.

[0055] The final waterborne polyurethane microfiber fabric has a rebound time of 30s.

[0056] By comparing Example 1 with Comparative Example 1, it can be seen that the simulated leather water-based polyurethane microfiber base fabric of Example 1 has a better feel, while the water-based polyurethane microfiber base fabric of Comparative Example 1 has a poorer feel. This is because the apparent density of the non-woven fabric of Comparative Example 1 is higher, and the sedimentation effect of the water-based polyurethane emulsion in the non-woven fabric is weak. Figure 2 As shown, the structure of continuously changing polyurethane distribution is still not obtained in the prepared waterborne polyurethane microfiber base cloth.

[0057] Comparative Example 2

[0058] A method for preparing a water-based polyurethane microfiber base cloth is basically the same as that in Example 1, except that the standing time in step (3) is 100 minutes.

[0059] The longitudinal cross-sectional diagram of the finally obtained waterborne polyurethane microfiber base fabric is as follows: Figure 3 As shown, the rebound time of the water-based polyurethane microfiber base fabric is 26s.

[0060] By comparing Example 1 with Comparative Example 2, it can be seen that the simulated leather water-based polyurethane microfiber base fabric of Example 1 has a better feel, while the water-based polyurethane microfiber base fabric of Comparative Example 2 has a poorer feel. This is because the standing time is too long, resulting in serious sinking of the water-based polyurethane resin in the non-woven fabric, and the distribution is concentrated on one side of the non-woven fabric, such as Figure 3 As shown, the structure of continuously changing polyurethane distribution is not obtained in the prepared waterborne polyurethane microfiber base fabric.

[0061] Comparative Example 3

[0062] A method for preparing a water-based polyurethane microfiber base cloth is basically the same as that in Example 1, except that the standing time in step (3) is 10 minutes.

[0063] The longitudinal cross-sectional diagram of the finally obtained waterborne polyurethane microfiber base fabric is as follows: Figure 4 As shown, the rebound time of the water-based polyurethane microfiber base fabric is 38s.

[0064] By comparing Example 1 with Comparative Example 3, it can be seen that the simulated leather water-based polyurethane microfiber base fabric of Example 1 has a better feel, while the water-based polyurethane microfiber base fabric of Comparative Example 3 has a worse feel. This is because the standing time is insufficient, resulting in the water-based polyurethane resin not settling significantly in the non-woven fabric. Figure 4 As shown, the structure of continuously changing polyurethane distribution is not obtained in the prepared waterborne polyurethane microfiber base fabric.

[0065] Comparative Example 4

[0066] A method for preparing a water-based polyurethane microfiber base cloth is basically the same as that in Example 1, except that: in step (2), the liquid content of the water-based polyurethane impregnating material is 280%, and on the premise of ensuring that the final resin content is consistent, the solid content of the impregnating liquid is prepared to be 15.5%, and the dynamic viscosity of the impregnating liquid at a temperature of 25°C is about 5mPa·s.

[0067] The longitudinal cross-sectional diagram of the finally obtained waterborne polyurethane microfiber base fabric is as follows: Figure 5 As shown, the rebound time of the water-based polyurethane microfiber base fabric is 32s.

[0068] By comparing Example 1 with Comparative Example 4, it can be seen that the simulated leather water-based polyurethane microfiber base fabric of Example 1 has a better feel, while the water-based polyurethane microfiber base fabric of Comparative Example 4 has a poor feel. This is because the water-based polyurethane impregnation material has a high liquid rate, and there is no sufficient space in the non-woven fabric for the polyurethane emulsion to move and settle to form a stepped distribution, such as Figure 5 As shown, the structure of continuously changing polyurethane distribution is not obtained in the prepared waterborne polyurethane microfiber base fabric.

[0069] Comparative Example 5

[0070] A method for preparing a water-based polyurethane microfiber base fabric is basically the same as that in Example 1, except that: in step (2), the liquid content of the water-based polyurethane impregnating material is 100%, and on the premise of ensuring that the final resin content is consistent, the solid content of the impregnating liquid is prepared to be 43.5%, and the dynamic viscosity of the impregnating liquid at a temperature of 25°C is about 6mPa·s.

[0071] The longitudinal cross-sectional diagram of the finally obtained waterborne polyurethane microfiber base fabric is as follows: Figure 6 As shown, the rebound time of the water-based polyurethane microfiber base fabric is 34s.

[0072] By comparing Example 1 with Comparative Example 5, it can be seen that the simulated leather water-based polyurethane microfiber base fabric of Example 1 has a better feel, while the water-based polyurethane microfiber base fabric of Comparative Example 5 has a poor feel. This is because the water-based polyurethane impregnation material has a low liquid rate and a small amount. After impregnation, the water-based polyurethane emulsion is more dispersed in the non-woven fabric, so that the polyurethane emulsion has no sufficient power to move and settle to form a stepped distribution, such as Figure 6 As shown, the structure of continuously changing polyurethane distribution is not obtained in the prepared waterborne polyurethane microfiber base fabric.

[0073] Example 2

[0074] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0075] (1) preparing waterborne polyurethane impregnated material;

[0076] The waterborne polyurethane impregnation material is prepared by mixing waterborne polyurethane emulsion YS-3000 produced by Dow Chemical (the solid content of polyurethane resin in the emulsion is 54%) and NaCl aqueous solution with a mass concentration of 2.3wt%. During the preparation process, the NaCl aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 31%. The mass proportion of the NaCl aqueous solution in the waterborne polyurethane impregnation material is 42.6%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 12mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0077] (2) The nonwoven fabric is a PX / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd. with an apparent density of 0.245 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 165%, and obtaining a wet fabric with a polyurethane resin content of 33.8wt%;

[0078] (3) Place the wet cloth horizontally on the platform and let it stand for 40 minutes;

[0079] (4) heat treating the wet cloth after standing at 100° C. for 1 min to complete the curing of the waterborne polyurethane impregnation material;

[0080] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0081] The final prepared simulated leather water-based polyurethane microfiber base fabric has a rebound time of 60s.

[0082] Example 3

[0083] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0084] (1) preparing waterborne polyurethane impregnated material;

[0085] The waterborne polyurethane impregnation material is prepared by mixing waterborne polyurethane emulsion 204N (polyurethane resin solid content in the emulsion is 35%) produced by Hongdeli Resin Co., Ltd. and NaHCO3 aqueous solution with a mass concentration of 0.8wt%. During the preparation process, the NaHCO3 aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 25%. The mass proportion of the NaHCO3 aqueous solution in the waterborne polyurethane impregnation material is 28.6%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 57mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0086] (2) The nonwoven fabric is a COPET / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd., with an apparent density of 0.254 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 150%, and obtaining a wet fabric with a polyurethane resin content of 27.3wt%;

[0087] (3) Place the wet cloth horizontally on the platform and let it stand for 42 minutes;

[0088] (4) heat treating the wet cloth at 94° C. for 1 min to complete the curing of the waterborne polyurethane impregnation material;

[0089] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0090] The final prepared simulated leather water-based polyurethane microfiber base fabric has a rebound time of 51s.

[0091] Example 4

[0092] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0093] (1) preparing waterborne polyurethane impregnated material;

[0094] The waterborne polyurethane impregnation material is prepared by mixing the waterborne polyurethane emulsion TF-678 (the solid content of the polyurethane resin in the emulsion is 35%) produced by Chuanhua Zhilian Co., Ltd. and a NaCl aqueous solution with a mass concentration of 1.5wt%. During the preparation process, the NaCl aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 21%. The mass proportion of the NaCl aqueous solution in the waterborne polyurethane impregnation material is 40%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 24mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0095] (2) The nonwoven fabric is a PX / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd. with an apparent density of 0.230 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 190%, and obtaining a wet fabric with a polyurethane resin content of 28.5wt%;

[0096] (3) Place the wet cloth horizontally on the platform and let it stand for 45 minutes;

[0097] (4) heat treating the wet cloth at 80° C. for 1.5 min to complete the curing of the waterborne polyurethane impregnation material;

[0098] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0099] The final prepared simulated leather water-based polyurethane microfiber base fabric has a rebound time of 51s.

[0100] Example 5

[0101] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0102] (1) preparing waterborne polyurethane impregnated material;

[0103] The waterborne polyurethane impregnation material is prepared by mixing waterborne polyurethane emulsion 204N (polyurethane resin solid content in the emulsion is 35%) produced by Hongdeli Resin Co., Ltd. and NaCl aqueous solution with a mass concentration of 1.8wt%. During the preparation process, the NaCl aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 23%. The mass proportion of the NaCl aqueous solution in the waterborne polyurethane impregnation material is 34.3%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 50mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0104] (2) The nonwoven fabric is a PX / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd. with an apparent density of 0.26 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 240%, and obtaining a wet fabric with a polyurethane resin content of 35.6wt%;

[0105] (3) Place the wet cloth horizontally on a platform and let it stand for 74 minutes;

[0106] (4) heat treating the wet cloth at 80° C. for 2 min to complete the curing of the waterborne polyurethane impregnation material;

[0107] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0108] The final prepared simulated leather water-based polyurethane microfiber base fabric has a rebound time of 52s.

[0109] Example 6

[0110] A method for preparing a simulated leather water-based polyurethane microfiber base fabric, the steps are as follows:

[0111] (1) preparing waterborne polyurethane impregnated material;

[0112] The waterborne polyurethane impregnation material is prepared by mixing the waterborne polyurethane emulsion TF-3906 (the solid content of the polyurethane resin in the emulsion is 35%) produced by Chuanhua Zhilian Co., Ltd. and the Na3PO4 aqueous solution with a mass concentration of 0.7wt%. During the preparation process, the Na3PO4 aqueous solution is added to the waterborne polyurethane emulsion until the solid content of the waterborne polyurethane impregnation material reaches 20%. The mass proportion of the Na3PO4 aqueous solution in the waterborne polyurethane impregnation material is 42.9%. The dynamic viscosity of the waterborne polyurethane impregnation material at a temperature of 25°C is 28mPa·s. The obtained waterborne polyurethane impregnation liquid can be completely gelled and solidified when placed horizontally with a thickness of 2mm and left standing at 80°C for 1min, and loses fluidity.

[0113] (2) The nonwoven fabric is a COPET / PET type island nonwoven fabric produced by Shanghai Huafeng Microfiber Technology Co., Ltd., with an apparent density of 0.235 g / cm 3 , using a water-based polyurethane impregnated material to impregnate the sea-island fiber non-woven fabric, controlling the liquid rate of the water-based polyurethane impregnated material to be 225%, and obtaining a wet fabric with a polyurethane resin content of 31wt%;

[0114] (3) Place the wet cloth horizontally on the platform and let it stand for 35 minutes;

[0115] (4) heat treating the wet cloth after standing at 90° C. for 2 min to complete the curing of the waterborne polyurethane impregnation material;

[0116] (5) drying the base fabric after the water-based polyurethane is cured, and removing the sea phase through a weight reduction process to obtain the simulated leather water-based polyurethane microfiber base fabric.

[0117] The final prepared simulated leather water-based polyurethane microfiber base fabric has a rebound time of 53s.

Claims

1. A method for preparing a simulated leather water-based polyurethane microfiber base fabric, characterized in that: The following steps are involved: (1) Preparation of waterborne polyurethane impregnation material; The dynamic viscosity μ of the waterborne polyurethane impregnation material at 25°C is 5-57mPa·s; (2) Use water-based polyurethane impregnation material with an apparent density of ρ of 0.23-0.26g / cm 3 The sea-island fiber nonwoven fabric is prepared by controlling the liquid rate of the waterborne polyurethane impregnated material to be 150-240% to obtain a wet fabric; (3) Place the wet cloth horizontally on the platform and let it stand for t min, t=a×(475ρ-65)±15; when μ is (1-20]mPa•s, a=0.99; when μ is (21-40]mPa•s, a=1; when μ is (40-60]mPa•s, a=1.01; (4) Control the waterborne polyurethane impregnation material on the wet cloth to solidify within 1 minute after standing; (5) After drying, the sea phase is removed by reducing the amount to obtain a simulated leather water-based polyurethane microfiber base fabric; In step (1), the waterborne polyurethane impregnation material mainly consists of an electrolyte-sensitive waterborne polyurethane emulsion and a monovalent electrolyte solution with a mass concentration of 0.7-2.3%, the mass proportion of the monovalent electrolyte solution in the waterborne polyurethane impregnation material is ≥15wt%, the solid content of the waterborne polyurethane impregnation material and the liquid carrying rate of the waterborne polyurethane impregnation material are coordinated to ensure that the waterborne polyurethane content in the sea island fiber non-woven fabric in step (2) is 27%-36%, and the waterborne polyurethane content in the sea island fiber non-woven fabric is % = (solid content of waterborne polyurethane impregnation material × liquid carrying rate of waterborne polyurethane impregnation material) / (solid content of waterborne polyurethane impregnation material × liquid carrying rate of waterborne polyurethane impregnation material + 1).

2. The method for preparing a simulated leather waterborne polyurethane microfiber base fabric according to claim 1, characterized in that: In step (4), the curing is performed by heat treatment, the heat treatment temperature is above 80° C., and the heat treatment time is at least 1 minute.

3. The method for preparing a simulated leather waterborne polyurethane microfiber base fabric according to claim 1, characterized in that: In step (2), the apparent density ρ of the sea island fiber nonwoven fabric is 0.24-0.245 g / cm 3 .

4. The method for preparing a simulated leather waterborne polyurethane microfiber base fabric according to claim 1, characterized in that: In step (2), the sea phase in the sea island fiber nonwoven fabric is a water-soluble polyester.

5. The method for preparing the simulated leather waterborne polyurethane microfiber base fabric according to claim 4, characterized in that: In step (5), the reduction is carried out by using alkali or water.

6. The method for preparing a simulated leather waterborne polyurethane microfiber base fabric according to claim 1, characterized in that: The rebound time of the simulated leather water-based polyurethane microfiber base fabric is 50~64s.