A high-pressure resistant reinforced steel wire composite pipe and production method thereof

By flanging the ends of the composite pipe and fixing the steel wire layer with inner and outer clamping fittings, the problem of wire pull-out in traditional high-pressure resistant reinforced steel wire composite pipes is solved, achieving higher pressure resistance and connection reliability.

CN116006787BActive Publication Date: 2024-11-22KANGTAI PLASTIC SCI & TECH GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310007024.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-11-22
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

Traditional high-pressure resistant reinforced steel wire composite pipes suffer from wire pull-out during use, leading to unstable connections.

Method used

Flanging is performed on both ends of the composite pipe, and the flanges are tightened from the inside and outside using first and second clamping parts. The pipe joint is formed by cold forming and hot-melt injection molding to fix the steel wire layer and prevent the steel wire from pulling.

Benefits of technology

It improves the pressure resistance and reliability of pipe connections, reduces the risk of wire breakage, and enhances the stability and sealing of the connection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116006787B_ABST
    Figure CN116006787B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of composite pipe forming, and discloses a high-pressure resistant reinforced steel wire composite pipe, including a composite pipe body, a first buckling piece, a second buckling piece, and a pipe joint. The connecting end of the composite pipe body is folded from the inside to the outside to form a flanging part; the first buckling piece is clamped on the composite pipe body, and the flanging part is crimped on the first buckling piece; the second buckling piece is clamped on the outside of the flanging part; the pipe joint is arranged at the connecting end of the composite pipe body and covers the flanging part. A production method of a composite pipe is also disclosed, including the steps of: fixing the composite pipe to be processed; sleeve the first buckling piece on the port side close to the composite pipe, cold-flanging the flanging part to compact the first buckling piece; sleeve the second buckling piece on the outside of the flanging part, and use a buckling mold to buckle the first buckling piece, the flanging part, and the second buckling piece; heat the flanging part to a hot melt state; and injection mold the pipe joint at the flanging part. The present application solves the problem of wire drawing in traditional high-pressure resistant reinforced steel wire composite pipes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite pipe forming, and in particular to a high-pressure resistant reinforced steel wire composite pipe and a production method thereof. Background Art

[0002] Composite pipes are pipes based on a composite structure of metal and thermoplastics, lined with non-metallic materials such as polypropylene, polyethylene or welded cross-linked polyethylene on the outside, and have the advantages of both metal pipes and non-metallic pipes.

[0003] High-pressure resistant reinforced steel wire composite pipe is made of high-strength plasticized steel wire mesh skeleton and thermoplastic polyethylene as raw materials. The steel wire winding mesh is used as the skeleton reinforcement of the polyethylene plastic pipe. High-performance HDPE modified adhesive resin is used to tightly connect the steel wire skeleton with the inner and outer layers of high-density high-performance polyethylene, giving it an excellent composite effect.

[0004] However, the performance of high-pressure resistant reinforced steel wire composite pipes is not stable enough. For example, wire drawing may occur during actual use. Summary of the invention

[0005] The main purpose of the present application is to provide a high-pressure resistant reinforced steel wire composite pipe and a production method thereof, aiming to solve the technical problem of steel wire drawing existing in the traditional high-pressure resistant reinforced steel wire composite pipe.

[0006] The technical solutions adopted in this application are as follows:

[0007] The first aspect provides:

[0008] A high-pressure resistant reinforced steel wire composite pipe, comprising:

[0009] A composite pipe body, wherein the connecting end of the composite pipe body is folded from inside to outside to form a flange portion;

[0010] a first buckling piece, the first buckling piece is clamped tightly on the composite pipe body, and the flange portion is crimped on the first buckling piece;

[0011] a second buckling piece, the second buckling piece being clamped tightly on the outer side of the flange portion;

[0012] A pipe joint is arranged at the connecting end of the composite pipe body and covers the flange portion.

[0013] Optionally, the composite pipe body includes a PE core pipe layer, a steel wire layer and a PE skin layer which are coated layer by layer from the inside to the outside.

[0014] Optionally, the outer diameter of the pipe joint is larger than the maximum outer diameter of the flanging portion.

[0015] Optionally, the first buckling piece and the second buckling piece are both ring structures.

[0016] The second aspect provides:

[0017] A method for producing a high-pressure resistant reinforced steel wire composite pipe comprises the following steps:

[0018] S1. Fix the composite pipe to be processed;

[0019] S2, sleeve a first buckling piece on the port side close to the composite pipe, and buckle the first buckling piece with a buckling mold;

[0020] S3, cold-rolling to form a flanged portion, and compacting the flanged portion again;

[0021] S4, sleeve a second buckling piece on the outer side of the flange portion, and use a buckling mold to buckle the first buckling piece, the flange portion and the second buckling piece for a second time;

[0022] S5, heating the flange portion to a hot melt state;

[0023] S6. Injection molding a pipe joint at the flanged portion.

[0024] Optionally, in step S2, the distance between the first buckling piece and the port steel wire layer of the composite pipe body is 0.5-1 times the wall thickness of the pipe body.

[0025] Optionally, the pressing depth of the first pressing member and the second pressing member is 1mm-4mm into the surface.

[0026] Optionally, in steps S2 and S4, before using the crimping die to fasten the first crimping piece, the flange portion and the second crimping piece, a crimping liner core needs to be inserted into the composite pipe.

[0027] Optionally, the insertion depth of the press-fit lining core is greater than the length of the flange portion, and the press-fit lining core fits against the inner wall of the composite tube.

[0028] Optionally, in step S5, the flange portion is heated to a hot melt state, wherein the heating temperature is 120° C.-160° C. and the heating time is 1 min-2 min.

[0029] Compared with the prior art, the beneficial effects of this application are:

[0030] First aspect:

[0031] The embodiment of the present application proposes a high-pressure resistant reinforced steel wire composite pipe, which is achieved by flanging the two ends of the pipe body, and after the ports on both sides of the pipe are folded, a first clamping piece and a second clamping piece are used to clamp the flanged parts inside and outside respectively, and the steel wire is fixed under the clamping pressure of the first clamping piece and the second clamping piece, thereby reducing the risk of wire drawing and greatly improving the pressure bearing capacity of the pipe connection.

[0032] Second aspect:

[0033] The production method of the high-pressure resistant reinforced steel wire composite pipe proposed in the embodiment of the present application has a simple process flow, uses a cold-flanging process to complete the port flanging, and uses a clamping die under the action of hydraulic pressure to clamp and fix the steel wire with two clamping parts, thereby reducing the risk of wire drawing and greatly improving the pressure bearing capacity of the pipe connection. In addition, the flanging port is plastic-encapsulated, and the connection method is hot-melt butt-jointing. Under the conditions of medium and high pressure transportation inside the pipe, there is no metal connection, which improves the reliability of the connection part. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic diagram of the sample tube flanging process in the embodiment of the present application;

[0035] Figure 2 This is a schematic cross-sectional view of a sample tube after flanging in an embodiment of the present application;

[0036] Figure 3 This is a cross-sectional schematic diagram of a flanging die in an embodiment of the present application;

[0037] Figure 4 This is a schematic diagram of a one-time pressing process of a pipe after flanging forming in an embodiment of the present application;

[0038] Figure 5 This is a schematic cross-sectional view of a sample tube after one-time pressing and forming in an embodiment of the present application;

[0039] Figure 6 This is a schematic diagram of the secondary crimping process of the sample pipe in the embodiment of the present application;

[0040] Figure 7 This is a schematic diagram of the end face of the sample tube after secondary pressing and forming in the embodiment of the present application;

[0041] Figure 8 This is a schematic diagram of the heating state of the sample pipe after the flanging and pressing is completed in the embodiment of the present application;

[0042] Fig. 9 This is a schematic diagram of the state of the injection-molded pipe joint of the sample pipe in the embodiment of the present application;

[0043] Fig.10 This is a schematic diagram of the structure of a high-pressure resistant reinforced steel wire composite pipe provided in an embodiment of the present application.

[0044] Description of the reference numerals in the accompanying drawings:

[0045] 1-steel wire layer, 2-PE skin layer, 3-PE core tube layer, 4-first buckling piece, 5-flanging mold, 6-flanging part, 7-buckle mold, 8-buckle core lining, 9-second buckling piece, 10-heating mold, 11-injection molding mold, 12-injection molding mold cavity, 13-injection core mold, 14-pipe joint. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0047] It should be noted that all directional indications in the embodiments of the present application (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0048] In this application, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0049] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present application, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0050] See attached Fig.10As shown, the embodiment of the present application provides a high-pressure resistant reinforced steel wire composite pipe, including a composite pipe body, a first buckling piece 4, a second buckling piece 9 and a pipe joint 14, wherein:

[0051] The composite pipe body includes a PE core tube layer 3, a steel wire layer 1 and a PE skin layer 2. The PE core tube layer 3, the steel wire layer 1 and the PE skin layer 2 are coated layer by layer from the inside to the outside and are overmolded. The steel wire layer 1 serves as a skeleton to support the composite pipe body. The PE core tube layer 3 and the PE skin layer 2 are corrosion-resistant, have stable chemical properties and a long service life. The PE core tube layer 3 and the PE skin layer 2 are respectively coated on both sides of the steel wire layer 1 to isolate the steel wire layer 1 and prevent the steel wire layer 1 from oxidation and corrosion.

[0052] The connecting ends on both sides of the composite pipe body are folded 180° from the inner side of the pipe body to the outer side of the pipe body to form a flange portion 6. The first buckling piece 4 is clamped tightly on the outer wall of the composite pipe body and the inner side of the flange portion 6, and the first buckling piece 4 is close to the bend of the flange portion 6, and the second buckling piece 9 is clamped on the outer side of the flange portion 6 and close to the tail section of the flange portion 6. The first buckling piece 4 and the second buckling piece 9 are staggered, and the flange portion 6 and the composite pipe body are simply buckled together under the action of external pressure, so that the flange structure at both ends of the composite pipe body and the first buckling piece 4 and the second buckling piece 9 are used to fix and press the flange structure, so that the steel wire layer 1 is buckled and fixed, thereby reducing the risk of wire drawing.

[0053] Of course, as an implementation method, the first buckling member 4 and the second buckling member 9 both adopt a ring structure, such as an iron ring, which is easy to obtain materials, easy to make, and has controllable costs. At the same time, the iron ring has low plasticity and can firmly clamp the fixed position.

[0054] The pipe joint 14 is injection molded on the two port sides of the composite pipe body, and the pipe joint 14 is covered on the flange portion 6. The outer diameter of the pipe joint 14 is larger than the maximum outer diameter of the flange portion 6. It can be understood that plastic packaging is performed on the flange port of the composite pipe body, and the connection method is hot-melt butt welding. Under the condition of high-pressure transportation inside the pipe, there is no metal connection, which can improve the reliability of the connection part.

[0055] It can be obtained that the connection method of traditional high-pressure steel wire composite pipes mainly uses crimping parts to tighten the pipe port, then sleeves the flange, and uses bolts to connect. Traditional high-pressure steel wire composite pipes have the following disadvantages during use. First: crimping parts need to be placed on the inner wall of the composite pipe during crimping, which is susceptible to corrosion; second: under long-term high-pressure operation and long-term stress relaxation of plastic materials, it is easy to cause the flange sealing performance to weaken and cause leakage; third: the crimping parts are in direct contact with the liquid transported inside the pipe, which is easy to corrode and has a short service life; fourth: the cost is high and the connection process is complicated. Obviously, compared with the high-pressure resistant reinforced steel wire composite pipe provided in the embodiment of the present application, the high-pressure resistant reinforced steel wire composite pipe provided in the embodiment of the present application has at least the following advantages:

[0056] First: by flanging the two side ports of the composite pipe from the inside to the outside, and setting the first buckle 4 on the outer wall of the composite pipe body and the inner side of the flanging part 6, and the second buckle 9 on the outer side of the flanging part 6, it is obvious that the first buckle 4 and the second buckle 9 are no longer located on the inner wall of the composite pipe body, and the probability of corrosion is greatly reduced.

[0057] Second: by flanging the two side ports of the composite pipe from the inside out, and limiting and fixing the flanging by the first buckling piece 4 and the second buckling piece 9, the wire drawing phenomenon can be effectively prevented.

[0058] Third: After the pipe is flanging, the flanging portion 6 is heated and hot-melted, and the pipe joint 14 is formed by injection molding instead of using a flange as a connecting piece. After hot-melt butt welding, the composite pipe body and the pipe joint 14 have good sealing and strong bearing capacity. Under the conditions of medium and high pressure transportation inside the pipe, there is no metal connection, which improves the reliability of the connection part.

[0059] The present application also provides a method for producing a high-pressure resistant reinforced steel wire composite pipe, comprising the following steps:

[0060] S1. Fixing the composite pipe body to be processed;

[0061] S2, sleeve a first buckling piece on the port side close to the composite pipe body, and buckle the first buckling piece with a buckling mold;

[0062] S3, cold-rolling to form a flanged portion, and compacting the flanged portion again;

[0063] S4, sleeve a second buckling piece on the outer side of the flange portion, and use a buckling mold to buckle the first buckling piece, the flange portion and the second buckling piece for a second time;

[0064] S5, heating the flange portion to a hot melt state;

[0065] S6. Injection molding a pipe joint at the flanged portion.

[0066] Specifically for each step:

[0067] Regarding step S1, fixing the composite pipe body to be processed;

[0068] It is conceivable that in order to prevent the composite pipe from rotating and shifting in the subsequent process, the composite pipe is fixed by a fixture or the like. Of course, there are various fixture structures, and the purpose is to clamp and fix the composite pipe. It is understandable that the fixture may be a three-turn chuck, a clamp, a pipe clamp, or the like.

[0069] Regarding step S2, a first buckling piece is sleeved on the port side close to the composite pipe body, and the first buckling piece is buckled with a buckling mold;

[0070] As a specific implementation method, the first buckling piece is an iron ring with a wall thickness of 2mm-4mm. The first buckling piece is fixed to the outer wall of the composite tube body, and the length from the port of the composite tube body is greater than the thickness of the composite tube body by 2mm-10mm. The specific position is adjusted according to the thickness of the composite tube body. The thicker the composite tube body, the farther the first buckling piece is from the port. Conversely, the thinner the composite tube body, the closer the first buckling piece is to the port. The reason is: the thicker the composite tube, the larger the span required at the bending point when folding, so a larger length needs to be reserved to complete the 180° flanging, so the first buckling piece needs to be placed slightly farther away.

[0071] Regarding step S3: cold-rolling to form a flanged portion, and compacting the flanged portion again;

[0072] After the first buckling piece is fixed in position, a flanging die is used to perform a cold flanging process on the composite pipe body port in a forming cavity of the flanging die under the action of a high axial hydraulic pressure, so that the composite pipe body is flanging 180 degrees.

[0073] Of course, as is well known in the art, the flanging die utilizes a stamping process to fold the workpiece along a certain curve and in a certain direction to form a flanging. According to the shape to be formed, a corresponding forming cavity is set to achieve flanging of different shapes.

[0074] Regarding step S4, a second buckling piece is sleeved on the outer side of the flange portion, and a buckling mold is used to buckle the first buckling piece, the flange portion and the second buckling piece for a second time;

[0075] It can be understood that in order to prevent the flange portion from curling up, the second buckling piece is clamped at one end of the flange portion close to the tail of the flange portion, and the second buckling piece is also an iron ring.

[0076] It should be pointed out that: no matter it is the first crimping or the second crimping, the crimping mold applies an annular pressure of not less than 20Mpa to the composite pipe body. During crimping, a crimping liner is inserted into the composite pipe body, wherein the insertion length of the crimping liner is greater than the length of the flanging part. The outer diameter of the crimping liner fits the inner wall of the composite pipe body to prevent the pipe from shrinking due to the crimping pressure. After crimping, the flanging part and the PE cortex of the pipe body are tightly connected without any gap.

[0077] Regarding step 5, heating the flange portion to a hot melt state;

[0078] It can be understood that as an effective implementation method: use a heating mold to uniformly heat the crimped and flanging port, the heating core needs to be close to the inner wall of the pipe, the heating part of the crimped and flanging port includes the flanging part, the composite pipe body port and the composite pipe body flanging after crimping, and the joint is extended by 5-10cm from the composite pipe body. The heating temperature is 120℃-160℃, the heating time is 1-2min, so that the heated part reaches a molten state, and the temperature of the molten part is measured by a temperature gun, and the temperature reaches at least 90℃.

[0079] In step S6, the pipe joint is injection molded at the flange portion.

[0080] It is understandable that in order to avoid the traditional connection method of using flanges as pipe fittings, the pipe joints are formed at the flanging part by injection molding. After hot-melt butt welding, the composite pipe body and the pipe joints have good sealing and strong bearing capacity. Under the conditions of medium and high pressure transportation inside the pipe, there is no metal connection, which improves the reliability of the connection parts.

[0081] In conjunction with the production method of the high pressure resistant reinforced steel wire composite pipe provided in the embodiment of the present application, see Figures 1 to 9 This content takes the production of a composite pipe body with a size of 5.0 cm as an example to provide the actual process flow of producing a high-pressure resistant reinforced steel wire composite pipe. Specifically:

[0082] First, a composite tube body with a size of 5.0 cm (hereinafter referred to as a sample tube) is taken and effectively fixed by a machine tool and a fixture to prevent the sample tube from being displaced during the forming process;

[0083] Next, see Figures 1 to 3 As shown, the sample pipe is folded 180° along the position of the first buckle 4 using a flanging die 5, and the first buckle 4 (i.e., an iron ring) is fixed to the outer wall of the PE cortex 2 of the sample pipe, and the distance between the first buckle 4 and the port is greater than 2mm of the pipe thickness;

[0084] Then, see Figure 4As shown, the flange part 6 is subjected to a crimping process in a crimping die 7, and the crimping die 7 applies a 25Mpa circumferential force to the sample pipe port. During crimping, a crimping liner 8 is inserted into the sample pipe, and the insertion length of the crimping liner 8 is greater than the crimping length of the flange part 6. The outer diameter of the crimping liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the crimping pressure. After crimping, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0085] Next, see Figures 5 to 7 As shown, the second buckling piece 9 is fixed on the outer surface of the flange part 6, and the second buckling piece 9 is located on the upper part of the steel wire layer of the flange part; the buckling mold 7 is used to buckle the second buckling piece 9 for the second time, and the second buckling piece 9 is embedded into the inner skin of the flange part 6 to fix the steel wire. Of course, the buckling liner 8 is inserted into the sample pipe during buckling, and the insertion length of the buckling liner 8 is greater than the buckling length of the flange part 6. The outer diameter of the buckling liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the buckling pressure. After buckling, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0086] Then, see Figure 8 As shown, the heated mold 10 is used to uniformly heat the crimped flange part 6, the heating core needs to be close to the inner wall of the sample pipe, the heated part of the crimped flange port includes the flange part, the pipe port and the pipe body flange, and the joint after crimping is extended by 5-10cm to form a composite pipe body, the heating temperature is 120℃, the heating time is 1min, so that the heated part reaches a molten state, and the temperature gun measures the molten part, and the measuring temperature is 90℃;

[0087] Finally, see Fig. 9 As shown, when the flange part is heated to a molten state, the sample pipe is quickly pulled out of the heating mold 10, and the injection core mold 13 is inserted into the heated flanged and buckled pipe. The inner core fits the inner wall of the PE core tube layer 3, and the port end face of the flange part is 20 mm away from the sealing end face of the injection molding mold cavity 12. The injection molding mold 11 is closed, and the flanged and buckled pipe is clamped and fixed by the injection molding mold 11. The injection molding mold 11 is internally injected, and the injected molten material liquid wraps the flange part 6, and finally the pipe joint 14 is formed, and the high-pressure resistant reinforced steel wire composite pipe of the present invention is formed.

[0088] Of course, this embodiment also provides a process flow for actually producing a high-pressure resistant reinforced steel wire composite pipe, taking the production of a composite pipe body with a size specification of 9.0 cm as an example.

[0089] First, a composite tube body with a size of 9.0 cm (hereinafter referred to as a sample tube) is taken and effectively fixed by a machine tool and a fixture to prevent displacement of the sample tube during the forming process;

[0090] Next, see Figures 1 to 3As shown, the sample pipe is folded 180° along the position of the first buckle 4 by using a flanging die 5; the first buckle 4 (i.e., an iron ring) is fixed on the outer wall of the PE cortex 2 of the sample pipe, and the distance between the first buckle 4 and the port is greater than 4 mm of the pipe thickness;

[0091] Then, see Figure 4 As shown, the flange part 6 is subjected to a crimping process in a crimping die 7, and the crimping die 7 applies a 30Mpa circumferential force to the sample pipe port. During crimping, a crimping liner 8 is inserted into the sample pipe, and the insertion length of the crimping liner 8 is greater than the crimping length of the flange part 6. The outer diameter of the crimping liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the crimping pressure. After crimping, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0092] Next, see Figures 5 to 7 As shown, the second buckling piece 9 is fixed on the outer surface of the flange part 6, and the second buckling piece 9 is located on the upper part of the steel wire layer of the flange part; the buckling mold 7 is used to buckle the second buckling piece 9 for the second time, and the second buckling piece 9 is embedded into the inner skin of the flange part 6 to fix the steel wire. Of course, the buckling liner 8 is inserted into the sample pipe during buckling, and the insertion length of the buckling liner 8 is greater than the buckling length of the flange part 6. The outer diameter of the buckling liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the buckling pressure. After buckling, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0093] Then, see Figure 8 As shown, the heated mold 10 is used to uniformly heat the crimped flange part 6, the heating core needs to be close to the inner wall of the sample pipe, the heated part of the crimped flange port includes the flange part, the pipe port and the pipe body flange after crimping, and the joint is extended by 5-10cm to form a composite pipe body, the heating temperature is 130℃, the heating time is 1.5min, so that the heated part reaches a molten state, and the temperature gun measures the molten part, and the measuring temperature is 90℃;

[0094] Finally, see Fig. 9 As shown, when the flange part is heated to a molten state, the sample pipe is quickly pulled out of the heating mold 10, and the injection core mold 13 is inserted into the heated flanged and buckled pipe. The inner core fits the inner wall of the PE core tube layer 3, and the port end face of the flange part is 20 mm away from the sealing end face of the injection molding mold cavity 12. The injection molding mold 11 is closed, and the flanged and buckled pipe is clamped and fixed by the injection molding mold 11. The injection molding mold 11 is internally injected, and the injected molten material liquid wraps the flange part 6, and finally the pipe joint 14 is formed, and the high-pressure resistant reinforced steel wire composite pipe of the present invention is formed.

[0095] In addition, this embodiment also provides a process flow for actually producing a high-pressure resistant reinforced steel wire composite pipe, taking the production of a composite pipe body with a size specification of 14.0 cm as an example.

[0096] First, a composite tube body with a size of 14.0 cm (hereinafter referred to as a sample tube) is taken and effectively fixed by a machine tool and a fixture to prevent displacement of the sample tube during the forming process;

[0097] Next, see Figures 1 to 3 As shown, the sample pipe is folded 180° along the position of the first buckle 4 using a flanging die 5, and the first buckle 4 (i.e., an iron ring) is fixed to the outer wall of the PE cortex 2 of the sample pipe, and the distance between the first buckle 4 and the port is greater than 8 mm of the pipe thickness;

[0098] Then, see Figure 4 As shown, the flange part 6 is subjected to a crimping process in a crimping die 7, and the crimping die 7 applies a 40Mpa circumferential force to the sample pipe port. During crimping, a crimping liner 8 is inserted into the sample pipe, and the insertion length of the crimping liner 8 is greater than the crimping length of the flange part 6. The outer diameter of the crimping liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the crimping pressure. After crimping, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0099] Next, see Figures 5 to 7 As shown, the second buckling piece 9 is fixed on the outer surface of the flange part 6, and the second buckling piece 9 is located on the upper part of the steel wire layer of the flange part; the buckling mold 7 is used to buckle the second buckling piece 9 for the second time, and the second buckling piece 9 is embedded into the inner skin of the flange part 6 to fix the steel wire. Of course, the buckling liner 8 is inserted into the sample pipe during buckling, and the insertion length of the buckling liner 8 is greater than the buckling length of the flange part 6. The outer diameter of the buckling liner 8 fits the inner wall of the PE core pipe layer 3 to prevent the pipe from shrinking due to the buckling pressure. After buckling, the flange part 6 and the PE skin layer 2 are tightly connected without any gap.

[0100] Then, see Figure 8 As shown, the heated mold 10 is used to uniformly heat the flanged portion 6, the heating core needs to be close to the inner wall of the sample pipe, the heated portion of the flanged port includes the flanged portion, the pipe port and the pipe body flanged seam after the flange is buckled and pressed, and the composite pipe body is extended by 5-10cm. The heating temperature is 150°C, the heating time is 2 minutes, and the heated portion is melted. The temperature gun measures the melted portion, and the measuring temperature is 90°C.

[0101] Finally, see Fig. 9As shown, when the flange part is heated to a molten state, the sample pipe is quickly pulled out of the heating mold 10, and the injection core mold 13 is inserted into the heated flanged and buckled pipe. The inner core fits the inner wall of the PE core tube layer 3, and the port end face of the flange part is 20 mm away from the sealing end face of the injection molding mold cavity 12. The injection molding mold 11 is closed, and the flanged and buckled pipe is clamped and fixed by the injection molding mold 11. The injection molding mold 11 is internally injected, and the injected molten material liquid wraps the flange part 6, and finally the pipe joint 14 is formed, and the high-pressure resistant reinforced steel wire composite pipe of the present invention is formed.

[0102] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A high pressure resistant reinforced steel wire composite pipe, characterized in that: include: A composite pipe body, wherein the connecting end of the composite pipe body is folded from the inside to the outside to form a flange portion, wherein the composite pipe body comprises a PE core pipe layer, a steel wire layer and a PE skin layer which are coated layer by layer from the inside to the outside, and the PE core pipe layer, the steel wire layer and the PE skin layer are overmolded; A first buckling piece, the first buckling piece is clamped tightly on the outer wall of the composite pipe body and the inner side of the flange portion, and the first buckling piece is close to the bending part of the flange portion; A second buckling piece, the second buckling piece is clamped on the outer side of the flange part and close to the tail section of the flange part, the second buckling piece is staggered with the first buckling piece, and the first buckling piece and the second buckling piece buckle the flange part to the outer wall of the composite pipe body under the action of external force, so that the steel wire layer is buckled and fixed to reduce the risk of wire drawing, wherein the first buckling piece and the second buckling piece both adopt a ring structure; A pipe joint, wherein the pipe joint is injection molded at the connecting end of the composite pipe body when the flanging part is heated to a hot-melt state, and covers the flanging part, wherein the heating core used when heating the flanging part needs to be close to the inner wall of the pipe, and the heating area of ​​the flanging part includes the flanging part, the port of the composite pipe body and the composite pipe body extending 5-10cm from the joint after the flanging of the composite pipe body is buckled, the heating temperature is 120℃-160℃, the heating time is 1-2min, so that the heated part reaches a molten state, and the temperature of the molten part is measured by a temperature measuring gun, and the temperature reaches at least 90℃.

2. The high pressure resistant reinforced steel wire composite pipe according to claim 1, characterized in that: The outer diameter of the pipe joint is greater than the maximum outer diameter of the flanging portion.

3. The high pressure resistant reinforced steel wire composite pipe according to claim 1, characterized in that: The first buckling piece and the second buckling piece are both ring structures.

4. A method for producing a high-pressure resistant reinforced steel wire composite pipe according to any one of claims 1 to 3, characterized in that: Includes steps: S1. Fixing the composite pipe body to be processed; S2, sleeve a first buckling piece on the port side close to the composite pipe body, and buckle the first buckling piece with a buckling mold; S3, cold-rolling to form a flanged portion, and compacting the flanged portion again; S4, sleeve a second buckling piece on the outer side of the flange portion, and use a buckling mold to buckle the first buckling piece, the flange portion and the second buckling piece for a second time; S5, heating the flange portion to a hot melt state; S6. Injection molding a pipe joint at the flanged portion.

5. The method for producing a high-pressure resistant reinforced steel wire composite pipe according to claim 4, characterized in that: In the step S2, the distance between the first pressing piece and the end steel wire layer of the composite pipe body is 0.5-1 times the wall thickness of the pipe body.

6. The high-pressure resistant reinforced steel wire composite pipe and its production method according to claim 4, characterized in that: The buckling depth of the first buckling member and the second buckling member is 1mm-4mm into the surface.

7. The high-pressure resistant reinforced steel wire composite pipe and its production method according to claim 4, characterized in that: In the steps S2 and S4, before the crimping die is used to fasten the first crimping member, the flange portion and the second crimping member, a crimping liner core needs to be inserted into the composite pipe.

8. The high-pressure resistant reinforced steel wire composite pipe and the production method thereof according to claim 7, characterized in that: The insertion depth of the buckled liner core is greater than the length of the flange portion, and the buckled liner core is in contact with the inner wall of the composite pipe.

9. The high-pressure resistant reinforced steel wire composite pipe and the production method thereof according to claim 4, characterized in that: In the step S5, the flange portion is heated to a hot melt state, wherein the heating temperature is 120° C.-160° C. and the heating time is 1 min-2 min.