A hydrogenation catalyst system and its preparation method and application

Through the combined system of Pd/NiO-Al2O3 and Cu-Zn/SiO2 catalysts, the problems of high cost, large energy consumption and poor catalyst stability in the hydrogenation synthesis of 1,4-cyclohexanedimethanol are solved, and high efficiency and low The catalytic effect of cost is comparable to the high inverse ratio.

CN116020437BActive Publication Date: 2024-11-12YULIN ZHONGKE CLEAN ENERGY INNOVATION RES INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211664313.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-12
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

The existing hydrogenation synthesis of 1,4-cyclohexanedimethanol processes have problems such as high production costs, serious energy consumption and loss, poor catalyst stability, and low reverse ratio of target products.

Method used

Using a combination system of Pd/NiO-Al2O3 catalyst and Cu-Zn/SiO2 catalyst, the activity and stability of the catalyst are improved through the design of single-atom palladium-supported and nano-hollow structure, and the catalyst structure is optimized to improve the reaction efficiency.

Benefits of technology

It significantly reduces production costs, improves catalytic activity and selectivity, reduces energy consumption, and improves product inverse proportion, achieving efficient catalytic effect under milder conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020437B_ABST
    Figure CN116020437B_ABST
Patent Text Reader

Abstract

The present application discloses a hydrogenation catalyst system and its preparation method and application, wherein the hydrogenation catalyst system comprises a Pd / NiO‑Al2O3 catalyst and a Cu‑Zn / SiO2 catalyst; in the Pd / NiO‑Al2O3 catalyst, a single atom Pd is loaded on the NiO‑Al2O3 composite oxide; the Pd / NiO‑Al2O3 catalyst has a mesoporous structure; in the Cu‑Zn / SiO2 catalyst, Cu and Zn nanoparticles are loaded on SiO2; and the Cu‑Zn / SiO2 catalyst has a hollow eggshell structure. The hydrogenation catalyst system is applied to the preparation of 1,4‑cyclohexanedimethanol by two-step hydrogenation of dioctyl terephthalate, and has extremely high catalytic activity, stability and selectivity, simple steps, low cost, green and pollution-free, high utilization rate of active components, and good preparation repeatability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a hydrogenation catalyst system, a preparation method and an application thereof, and belongs to the field of continuous flow hydrogenation technology, and specifically to a catalyst used in the process of hydrogenating dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol, a preparation method and an application thereof. Background Art

[0002] 1,4-Cyclohexanedimethanol (CHDM), also known as 1,4-dihydroxymethylcyclohexane, is a white waxy solid. It is a symmetrical alicyclic diol containing two primary alcohol hydroxyl groups. It has two different structural formulas, trans and cis, with a melting point of 43°C (cis) and 70°C (trans), and a boiling point of 286°C. In industry, CHDM can be used to produce new important polyesters instead of ethylene glycol or other polyols. It has good thermal stability and thermoplasticity, and can maintain stable physical and electrical properties at high temperatures. In particular, the polyester modified with trans-CHDM has a high glass transition temperature and softening temperature, good chemical resistance and environmental adaptability, and a wide range of applications. This series of new polyester products can be made into high-performance plasticizers for glazes and coatings, and used to make special linear polyester fibers suitable for electrical equipment. In view of the fact that the comprehensive performance of trans-CHDM is better than that of cis-CHDM, the trans-cis ratio is an important research indicator in the preparation process of CHDM.

[0003] At present, CHDM is mainly produced commercially through a two-step hydrogenation process, using dimethyl terephthalate as a raw material. First, the benzene ring is hydrogenated to produce dimethyl 1,4-cyclohexanedicarboxylate, and then the dimethyl 1,4-cyclohexanedicarboxylate is further hydrogenated to produce CHDM. Eastman Company of the United States was the first to apply for relevant patents, and Eastman Company is still in a leading position in CHDM production technology. Patent CN102795965A discloses a two-step hydrogenation process for preparing CHDM, in which Ru / Al2O3 is used as a catalyst for the first step of benzene ring hydrogenation, and Cu-Cr catalyst is used in the second step. In the first step of the benzene ring hydrogenation production process published in patent CN1099745A, Pd / Al2O3 is used as a catalyst. Patent CN1060153C discloses the preparation of CHDM by catalyzing dimethyl 1,4-cyclohexanedicarboxylate in the presence of a manganese-assisted copper catalyst and then further hydrogenating it. Since dimethyl terephthalate is solid at room temperature, has a melting point of up to 140°C, and has very low solubility in various organic solvents, a large amount of solvent is required in the first stage of benzene ring hydrogenation, resulting in high cycle energy consumption. In the second stage ester hydrogenation process, a large amount of methanol circulating solvent is used, and the subsequent methanol separation energy consumption is also quite high. Patent CN110437033A discloses a method for preparing CHDM by a two-step hydrogenation method using liquid dioctyl terephthalate, dibutyl terephthalate, and didecyl terephthalate as raw materials, but the study did not explore the stability of the catalytic system and the product CHDM trans-cis ratio.

[0004] So far, reports on CHDM synthesis by hydrogenation show that the production process of CHDM still has problems such as high production cost, serious energy consumption, poor catalyst stability, low yield of target product and low reverse to direct ratio of CHDM in the product. Therefore, there is still a need to develop a catalyst system with low cost, high activity, high selectivity and good stability in the field of CHDM synthesis by hydrogenation. Summary of the invention

[0005] According to one aspect of the present application, a hydrogenation catalyst system is provided for synthesizing 1,4-cyclohexanedimethanol by a two-step hydrogenation process using dioctyl terephthalate as a raw material. The catalyst adopts a single-atom catalyst system, which can not only significantly reduce the precious metal loading, improve the utilization rate of metal atoms and reduce production costs, but also adjust the catalytic system through the micro-environment to improve stability in a specific reaction field; the catalyst also adopts a core-shell structure catalyst, which can achieve a good arrangement of the main active component and the auxiliary alloy shell layer in the microstructure, adjust the adsorption mode of the reactants through the catalyst structure, change the stereoselectivity of the product, and improve stability through structural confinement.

[0006] This application adopts the following technical solutions:

[0007] A hydrogenation catalyst system, comprising a Pd / NiO-Al2O3 catalyst and a Cu-Zn / SiO2 catalyst;

[0008] In the Pd / NiO-Al2O3 catalyst, single-atom Pd is loaded on the NiO-Al2O3 composite oxide;

[0009] In the Cu-Zn / SiO2 catalyst, Cu and Zn nanoparticles are loaded on SiO2.

[0010] In the Pd / NiO-Al2O3 catalyst, the content of the single-atom Pd is 0.1-2.0wt%;

[0011] Optionally, in the Pd / NiO-Al2O3 catalyst, the content of the single-atom Pd is selected from any value of 0.1wt%, 0.2wt%, 0.3wt%, 1wt%, 1.2wt%, 1.5wt%, 2.0wt%, or any range value between the two.

[0012] Optionally, in the Pd / NiO-Al2O3 catalyst, the content of the single-atom Pd is 0.3 to 1.0 wt%.

[0013] Optionally, in the Pd / NiO-Al2O3 catalyst, the content of the single-atom Pd is 0.5-0.7wt%.

[0014] In the Cu-Zn / SiO2 catalyst, the content of Cu is 10-50wt%, and the content of Zn is 1-10wt%.

[0015] Optionally, in the Cu-Zn / SiO2 catalyst, the content of Cu is selected from any value of 10wt%, 15wt%, 20wt%, 40wt%, 45wt%, 50wt%, or any range between the two.

[0016] Optionally, in the Cu-Zn / SiO2 catalyst, the content of Cu is 20 to 40 wt%.

[0017] Optionally, in the Cu-Zn / SiO2 catalyst, the Cu content is selected from any value of 25wt%, 27.5wt%, 30wt%, 32.5wt%, 35wt%, 37.5wt%, 40wt%, or any range value between the two.

[0018] Optionally, in the Cu-Zn / SiO2 catalyst, the Zn content is selected from any value of 1wt%, 2wt%, 3wt%, 8wt%, 9wt%, 10wt%, or any range value between the two.

[0019] Optionally, in the Cu-Zn / SiO2 catalyst, the content of Zn is 3 to 8 wt%.

[0020] Optionally, in the Cu-Zn / SiO2 catalyst, the Zn content is selected from any value of 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, or any range value between two of them.

[0021] Optionally, the Pd / NiO-Al2O3 catalyst has a mesoporous structure.

[0022] Optionally, the Cu-Zn / SiO2 catalyst is a hollow eggshell structure.

[0023] According to another aspect of the present application, a method for preparing the above-mentioned hydrogenation catalyst system is provided, comprising the following steps:

[0024] S1, impregnating NiO-Al2O3 in an impregnation solution containing a palladium source, and drying to obtain a Pd / NiO-Al2O3 catalyst;

[0025] S2. Add nano-silicon oxide balls into a mixed solution containing a copper source and a zinc source and place the mixture in a sealed container for reaction and calcination to obtain a Cu-Zn / SiO2 catalyst.

[0026] Optionally, in the step S1, the preparation of NiO-Al2O3 includes the following steps: S0, adding nickel nitrate to a raw material solution containing polyethylene glycol, P123, and anhydrous ethanol to obtain solution a, adding solution b containing aluminum isopropoxide, concentrated nitric acid, and anhydrous ethanol to solution a, heating to react, and roasting II to obtain NiO-Al2O3.

[0027] Optionally, in the preparation method of NiO-Al2O3, the raw material solution containing polyethylene glycol, P123 and anhydrous ethanol is prepared by dissolving polyethylene glycol and P123 in anhydrous ethanol and stirring at room temperature for 4 to 10 hours.

[0028] Optionally, in the preparation method of NiO-Al2O3, the solution a is prepared by adding nickel nitrate to a raw material solution containing polyethylene glycol, P123 and anhydrous ethanol, and stirring at room temperature for 8 to 12 hours.

[0029] Optionally, in the preparation method of NiO-Al2O3, the solution b is prepared by dissolving aluminum isopropoxide and concentrated nitric acid in anhydrous ethanol and stirring at room temperature for 4 to 10 hours.

[0030] Optionally, in the method for preparing NiO-Al2O3, after the solution b is added to the solution a, the mixture is stirred at room temperature for 18 to 36 hours.

[0031] Optionally, in the preparation method of NiO-Al2O3, the mass concentration of polyethylene glycol in the raw material solution a is 0.05-2.0 g / ml, and the mass concentration of P123 is 0.01-0.1 g / ml.

[0032] Optionally, in the preparation method of NiO-Al2O3, the mass concentration of aluminum isopropoxide in the solution b is 0.05-2.0 g / ml, and the mass concentration of nitric acid is 0.05-1.0 g / ml.

[0033] Optionally, in the preparation method of NiO-Al2O3, the reaction conditions are: reaction temperature is 40-70°C, and reaction time is 24-60h.

[0034] Optionally, in the preparation method of NiO-Al2O3, the calcination conditions are: calcination at 400-750°C for 4-10 hours.

[0035] Optionally, in step S1, the impregnation solution containing the palladium source further comprises concentrated hydrochloric acid and water.

[0036] Optionally, the concentration of the concentrated hydrochloric acid is 36% to 38%.

[0037] Optionally, the weight ratio of concentrated hydrochloric acid, water and palladium source in the impregnation solution containing the palladium source is (1-4):(100-750):1.

[0038] Optionally, the weight ratio of concentrated hydrochloric acid, water and palladium source in the impregnation solution containing the palladium source is (1-2):(100-300):1.

[0039] Optionally, in step S1, the palladium source is selected from at least one of palladium chloride, palladium nitrate and palladium acetate.

[0040] Optionally, in step S1, the immersion time is 8 to 36 hours.

[0041] Optionally, in step S1, the drying condition is: drying at 70-120° C. for 10-24 hours.

[0042] Optionally, the drying is vacuum drying.

[0043] During the preparation of Pd / NiO-Al2O3 catalyst, atomic-level nickel and aluminum vacancies are constructed on the surface of the composite oxide by combining organic templates, peptization conditions, and post-treatment conditions. Subsequently, single palladium atoms are loaded by utilizing the electronic interaction between the atomic-level vacancies on the surface of the nickel-aluminum composite oxide and the palladium species precursor. This not only improves the activity of the main active metal, but also enhances the ability to activate hydrogen through the strong interaction between the carrier and the palladium atoms, thereby improving the hydrogenation capacity of the benzene ring.

[0044] Optionally, in step S2, the nano silicon oxide spheres are prepared according to the preparation method in the document Chem. Mater., 2006, 18, 2733.

[0045] Optionally, in step S2, the copper source is selected from at least one of copper nitrate, copper chloride, and basic copper carbonate; the zinc source is selected from at least one of zinc nitrate, zinc chloride, and zinc acetate.

[0046] Optionally, in step S2, the mixed solution further comprises aqueous ammonia and water.

[0047] Optionally, the ammonia water is concentrated ammonia water; the concentration of the concentrated ammonia water is 22-25%.

[0048] Optionally, the weight ratio of the ammonia water, water to the copper source and zinc source in the mixed solution is (10-100):(300-1000):(2-12):1.

[0049] Optionally, the weight ratio of the ammonia water, water to the copper source and zinc source in the mixed solution is (10-100):(600-1000):(5-12):1.

[0050] Optionally, the step S2 includes adding the nano silicon oxide balls to a mixed solution containing a copper source, a zinc source, ammonia water and water, and then ultrasonically stirring the solution at room temperature for 3 to 10 hours.

[0051] Optionally, the step S2 further includes filtering after heating the reaction and washing with water for 3 to 5 times.

[0052] Optionally, the weight ratio of the nano silicon oxide spheres to the mixed solution is 1:100-400.

[0053] Optionally, in step S2, the conditions for the heating reaction are: reaction temperature is 140-180° C., and reaction time is 4-18 hours.

[0054] Optionally, in step S2, the calcination conditions of I are: calcination at 350-550° C. for 4-10 hours.

[0055] During the preparation of Cu-Zn / SiO2 catalyst, ammonia is used to coordinate and protect metal precursor salts to form caged ammonia-coordinated metal salt macromolecules in aqueous solution. Subsequently, ammonia aqueous solution is used to react the caged ammonia-coordinated metal salt macromolecules with nano-silicon oxide balls under ultrasonic and heating conditions, forming uniform Cu-O-Si or Zn-O-Si bonds between the metal and silicon oxide. Finally, after the reaction is completed, a CuZn bimetallic alloy is formed on the surface of the nano-silicon oxide balls, and the internal silicon oxide is continuously etched to form a hollow structure. Not only can a uniform alloy structure be formed on the catalyst surface to improve the uniform alloy interface and improve the catalyst performance; but the formation of the hollow structure can also obviously form special functions of hydrogen storage and activation in the microstructure, thereby improving the catalytic performance.

[0056] According to another aspect of the present application, there is also provided the use of at least one of the above hydrogenation catalyst system and the hydrogenation catalyst system obtained by the above preparation method in the two-step hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol.

[0057] Optionally, the application comprises the following steps:

[0058] 1) contacting dioctyl terephthalate with a Pd / NiO-Al2O3 catalyst, heating for reaction, and obtaining a raw material containing dioctyl 1,4-cyclohexanedicarboxylate;

[0059] 2) The raw material containing dioctyl 1,4-cyclohexanedicarboxylate obtained in step 1) is contacted with a Cu-Zn / SiO2 catalyst and heated for reaction to obtain 1,4-cyclohexanedimethanol.

[0060] Optionally, the step 1) and the step 2) further include activating the Pd / NiO-Al2O3 catalyst and the Cu-Zn / SiO2 catalyst in a hydrogen atmosphere or a mixed atmosphere of hydrogen and inert gas, respectively.

[0061] Optionally, the activation conditions of the Pd / NiO-Al2O3 catalyst are: reaction pressure of 0.05-0.3 MPa, gas space velocity of 30-1500 h -1 The activation temperature is 200-350°C, the heating rate is 0.5-5°C / min, and the activation time is 2-18h.

[0062] Optionally, the activation conditions of the Pd / NiO-Al2O3 catalyst are: reaction pressure of 0.1-0.2 MPa, gas space velocity of 30-1500 h -1 The activation temperature is 200-250°C, the heating rate is 0.5-5°C / min, and the activation time is 2-18h.

[0063] Optionally, the activation conditions of the Cu-Zn / SiO2 catalyst are: reaction pressure of 0.05-0.3 MPa, gas space velocity of 100-2000 h -1 The activation temperature is 180-350°C, the heating rate is 0.5-10°C / min, and the activation time is 3-38h.

[0064] Optionally, the activation conditions of the Cu-Zn / SiO2 catalyst are: reaction pressure of 0.1-0.2 MPa, gas space velocity of 100-2000 h -1 , the activation temperature is 250-300℃, the heating rate is 0.5-10℃ / min, and the activation time is 3-38h.

[0065] Optionally, in step 1), the conditions for the heating reaction are: reaction temperature is 130-220°C, reaction pressure is 2.0-8.0 MPa, and liquid hourly space velocity of dioctyl terephthalate is 0.01-3.5 h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 5 to 50:1.

[0066] Optionally, in step 2), the conditions for the heating reaction are: reaction temperature of 200-260° C., reaction pressure of 2.0-8.0 MPa, liquid hourly space velocity of dioctyl terephthalate of 0.01-2.0 h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 50-1000:1.

[0067] In this application, unless otherwise specified, the data range given is selected from any value in the range and includes the endpoint value of the range.

[0068] In the present application, normal temperature refers to 20 to 30°C.

[0069] The beneficial effects of this application include:

[0070] 1) The hydrogenation catalyst system provided in the present application includes a catalyst Pd / NiO-Al2O3 with a mesoporous structure of nickel-aluminum composite oxide loaded with single-atom Pd and a CuZn bimetallic alloy heterogeneous catalyst Cu-Zn / SiO2 with a nano hollow structure, which can achieve excellent catalytic effect in the hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol under relatively mild reaction conditions. It is firstly used in the catalytic two-step hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol, and has extremely high catalytic activity, stability and selectivity.

[0071] 2) The present application provides a method for preparing a hydrogenation catalyst system, wherein the Pd / NiO-Al2O3 catalyst first utilizes a template and a hydrolysis-gelling method to construct a nickel-aluminum composite oxide carrier with a mesoporous structure, and simultaneously during the carrier preparation process, an organic template, gelling conditions, post-treatment conditions, etc. are combined to adjust and construct atomic-level nickel and aluminum vacancies on the surface of the composite oxide; subsequently, the electronic interaction between the atomic-level vacancies on the surface of the nickel-aluminum composite oxide and the palladium species precursor is utilized to load palladium single atoms to construct a single-atom palladium-based catalyst. By controlling the surface vacancies during the carrier synthesis process and then utilizing the vacancies to prepare single-atom catalysts, the activity of the main active metal can be improved, and the ability to activate hydrogen can be enhanced through the strong interaction between the carrier and the palladium atoms, thereby improving the ability to hydrogenate the benzene ring. The Cu-Zn / SiO2 catalyst first prepares nano-silicon oxide balls, and then uses ammonia to coordinate and protect the metal precursor salt to form caged ammonia-coordinated metal salt macromolecules in an aqueous solution. Then, an ammonia solution is used to react the caged ammonia-coordinated metal salt macromolecules with the nano-silicon oxide balls under ultrasonic and heating conditions, forming a uniform Cu-O-Si or Zn-O-Si bond between the metal and the silicon oxide. Finally, after the reaction is completed, a CuZn bimetallic alloy is formed on the surface of the nano-silicon oxide balls, and the internal silicon oxide is continuously etched to form a hollow structure. Not only can a uniform alloy structure be formed on the catalyst surface to improve the uniform alloy interface and improve the catalyst performance, but the formation of the hollow structure can also obviously form special functions of hydrogen storage and activation in the microstructure, thereby improving the catalytic performance.

[0072] 3) The application of the hydrogenation catalyst system provided in the present application in the two-step hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol, the nickel-aluminum composite oxide loaded single atom catalyst with a mesoporous structure is combined with the CuZn bimetallic alloy multiphase catalyst with a nano hollow structure, the Pd / NiO-Al2O3 catalyst is used in the first step of the benzene ring hydrogenation reaction, and the Cu-Zn / SiO2 catalyst is used in the second step of the ester hydrogenation reaction. Liquid dioctyl terephthalate is used as the raw material. In the first step of the benzene ring hydrogenation reaction, no solvent is required, and the pure raw material can enter the reactor, which greatly reduces the reaction energy consumption; in the second step of the ester hydrogenation reaction, no solvent is required, which significantly reduces energy consumption and reduces production costs. The product mixture after the first step of the hydrogenation reaction does not need to be separated and directly enters the second step of the ester hydrogenation reactor, which can not only reduce the investment in fixed equipment, but also reduce the separation cost. In addition, the main by-product of the two-step hydrogenation of dioctyl terephthalate is octanol, which also has a huge market and can effectively improve the market economic value of the process.

[0073] 4) The preparation of the hydrogenation catalyst in the process method of the present application and the process of preparing 1,4-cyclohexanedimethanol by two-step hydrogenation thereof are simple in steps, low in cost, green and pollution-free, with high utilization rate of active components and good preparation repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 Transmission electron microscopy images (a) to (d) of different positions on the Pd / NiO-Al2O3 catalyst in the catalyst system prepared in Example 1 of the present invention, in which some Pd single atoms are indicated by yellow circles.

[0075] Figure 2 TEM images of the Cu-Zn / SiO2 catalyst in the catalyst system prepared in Example 1 of the present invention, wherein (a) is a nano-SiO2 sphere loaded with Cu-Zn nanoparticles, and (b) is a partial enlarged view of (a), and the black ones are Cu-Zn nanoparticles.

[0076] Figure 3 This is a graph showing the stability test data of the catalyst system in the first step reaction of Example 4 of the present invention.

[0077] Figure 4 This is a graph showing the stability test data of the catalyst system in the second step reaction of Example 4 of the present invention. DETAILED DESCRIPTION

[0078] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0079] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased through commercial channels.

[0080] As an embodiment, the present application uses a catalyst system to carry out two-step hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol using the following technical scheme:

[0081] The catalyst system includes: a Pd / NiO-Al2O3 catalyst for (1) hydrogenating dioctyl terephthalate to prepare 1,4-cyclohexane dioctyl ester, and a Cu-Zn / SiO2 catalyst for (2) hydrogenating 1,4-cyclohexane dioctyl ester to prepare 1,4-cyclohexanedimethanol. The Pd / NiO-Al2O3 catalyst for benzene ring hydrogenation is a single-atom Pd catalyst supported by a nickel-aluminum composite oxide, and the content of the single-atom Pd is 0.1-2.0% based on the mass of the Pd element; the Cu-Zn / SiO2 catalyst used in the ester hydrogenation reaction process is a catalyst with a hollow eggshell structure, and the content of Cu is 10-50% based on the mass of the Cu element, and the content of Zn is 1-10% based on the mass of the Zn element; the rest is a carrier.

[0082] Wherein, the Pd / NiO-Al2O3 catalyst in process (1) is prepared by the following steps:

[0083] (I) Dissolve polyethylene glycol and P123 in anhydrous ethanol and stir at room temperature for 4 to 10 hours. The mass concentration of the polyethylene glycol solution is 0.05 to 2.0 g / ml, and the mass concentration of P123 is 0.01 to 0.1 g / ml.

[0084] (II) then adding the calculated amount of nickel nitrate to the solution obtained in (I) and stirring for 8 to 12 hours;

[0085] (III) dissolving aluminum isopropoxide and concentrated nitric acid in anhydrous ethanol and stirring at room temperature for 4 to 10 hours, wherein the mass concentration of aluminum isopropoxide is 0.05 to 2.0 g / ml and the concentration of nitric acid is 0.05 to 1.0 g / ml;

[0086] (IV) adding the solution obtained in (III) to the solution obtained in (II) to obtain a mixed solution, and stirring at room temperature for 18 to 36 hours;

[0087] (V) heating the mixed solution obtained in (IV) at 40 to 70° C. for 24 to 60 hours to obtain a sample;

[0088] (VI) calcining the obtained sample in a muffle furnace at 400-750° C. for 4-10 hours to obtain a NiO-Al2O3 sample;

[0089] (VII) The NiO-Al2O3 sample obtained in step (VI) is immersed in a chloropalladic acid impregnation solution for 8 to 36 hours, and then dried at 70 to 120°C for 10 to 24 hours to obtain a Pd / NiO-Al2O3 catalyst.

[0090] (2) Process The Cu-Zn / SiO2 catalyst is prepared by the following steps:

[0091] (I) Preparation of nano-silicon oxide spheres according to the literature Chem. Mater., 2006, 18, 2733.

[0092] (II) dissolving Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and NH3.H2O in deionized water to form a uniform solution;

[0093] (III) Mix the nano-silicon oxide spheres prepared in (I) with the solution of (II), and stir them ultrasonically for 3 to 10 hours; then transfer the mixture to a heated reactor, and heat and react at 140 to 180°C for 4 to 18 hours under stirring conditions. After cooling, filter to obtain a solid sample, wash it with deionized water for 3 to 5 times, dry it at 80 to 120°C for 4 to 24 hours, and then calcine it at 350 to 550°C for 4 to 10 hours to obtain a Cu-Zn / SiO2 catalyst.

[0094] The use of the above catalyst in the process of preparing 1,4-cyclohexanedimethanol by two-step hydrogenation of dioctyl terephthalate comprises the following steps:

[0095] The first step is the benzene ring hydrogenation reaction. The Pd / NiO-Al2O3 catalyst in the catalyst system described in process (1) is loaded into the packed bed reactor No. 1. The catalyst is activated in hydrogen or a hydrogen-inert gas mixture before use. The activation conditions are: pressure of 0.05-0.3 MPa, gas space velocity of 30-1500 h -1 , the activation temperature is 200-350℃, the heating rate is 0.5-5℃ / min, and the activation time is 2-18h. After the activation is completed, the system is adjusted to the specified reaction conditions, and dioctyl terephthalate (DOTP) liquid raw material is pumped in. The reaction conditions are: temperature is 130-220℃, pressure is 2.0-8.0MPa, and the hourly space velocity of dioctyl terephthalate liquid is 0.01-3.5h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 5 to 50:1.

[0096] In the second step, ester hydrogenation reaction, the Cu-Zn / SiO2 catalyst in the catalyst system described in process (2) is loaded into the No. 2 packed bed reactor. The catalyst is activated in hydrogen or a hydrogen-inert gas mixture before use. The activation conditions are: pressure of 0.05-0.3 MPa, gas space velocity of 100-2000 h -1, the activation temperature is 180-350℃, the heating rate is 0.5-10℃ / min, and the activation time is 3-38h. After the activation is completed, the system is adjusted to the specified reaction conditions, and the liquid raw material of 1,4-cyclohexanedicarboxylic acid dioctyl ester (DOTCH) in the first step is pumped in to obtain the target product 1,4-cyclohexanedimethanol (CHDM). The reaction conditions are: temperature is 200-260℃, pressure is 2.0-8.0MPa, and the liquid hourly space velocity of dioctyl terephthalate is 0.01-2.0h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 50-1000:1.

[0097] Example 1

[0098] The first step is the preparation of benzene ring hydrogenation catalyst:

[0099] 2.0 g of polyethylene glycol and 1.5 g of P123 were dissolved in 30 mL of anhydrous ethanol, stirred at room temperature for 10 h, then 0.2 g of nickel nitrate was added to the above solution, stirred for 8 h, and solution A was obtained; 1.8 g of aluminum isopropoxide and 1.3 mL of concentrated nitric acid were dissolved in 20 ml of anhydrous ethanol, stirred at room temperature for 6 h, and solution B was obtained; solution B was poured into solution A, stirred at room temperature for 24 h to obtain a mixture; then the mixture was heated at 60 ° C for 48 h The sample was obtained; finally, the obtained sample was placed in a muffle furnace and calcined at 500°C for 4h to obtain a NiO-Al2O3 sample; 0.0152g of palladium chloride, 0.0183g of concentrated hydrochloric acid, and 3.8g of deionized water were weighed and mixed, and after stirring and dissolving, a chloropalladium acid impregnation solution was obtained, and 2.0g of the above NiO-Al2O3 sample was added thereto, impregnated at room temperature for 8 hours, and vacuum dried at 70°C for 3h to obtain a 1-Pd / NiO-Al2O3 catalyst sample. The product is shown in the attached Figure 1 As shown in the figure, it can be seen that the metal Pd is dispersed in the form of single atoms on the composite support NiO-Al2O3, forming a typical single atom catalyst

[0100] DD220827I

[0101] The second step ester hydrogenation catalyst preparation:

[0102] According to the method of preparing nano silicon oxide balls in the literature Chem. Mater., 2006, 18, 2733, 9 mL of concentrated ammonia water and 8 mL of ethyl orthosilicate were added to 25 mL of deionized water and stirred at 40°C for 2 hours. After centrifugation, the prepared silicon balls were washed with deionized water and ethanol for 3 times respectively, and then added to 60 ml of deionized water for use; 2.4 g of Cu(NO3) 2· 3H2O, 0.3g Zn(NO3) 2·6H2O and 12mL concentrated ammonia water were dissolved in 250mL deionized water to form a uniform solution; the nano-silicon oxide balls prepared above were mixed with the uniform solution and ultrasonically stirred for 4h; the mixture was then transferred to a heating reactor and heated at 140℃ for 8h under stirring conditions. After cooling, the solid sample was filtered, washed with deionized water 5 times, dried at 120℃ for 10h, and then calcined at 550℃ for 4h to obtain a 1-Cu-Zn / SiO2 catalyst sample. The product is shown in the attached Figure 2 (a) shows a hollow eggshell structure. In the local magnified image, it can be seen that Cu-Zn nanoparticles are dispersed on the SiO2 carrier. The acidity of the carrier provides an important anchoring point for the nanoparticles.

[0103] Two-step hydrogenation of dioctyl terephthalate to produce 1,4-cyclohexanedimethanol:

[0104] The 1-Pd / NiO-Al2O3 catalyst was loaded into the No. 1 packed bed reactor of the first step hydrogenation process. The catalyst was activated in hydrogen before use. The activation conditions were: pressure of 0.1 MPa, gas space velocity of 1000 h -1 , the activation temperature is 200℃, the heating rate is 2℃ / min, and the activation time is 4h. After the activation is completed, the system is adjusted to the specified reaction conditions, and dioctyl terephthalate (DOTP) liquid raw material is pumped in. The reaction conditions are: temperature is 150℃, pressure is 3.0MPa, and the hourly space velocity of dioctyl terephthalate liquid is 3.5h -1 , the molar ratio of hydrogen to dioctyl terephthalate was 30: 1. The conversion of dioctyl terephthalate (DOTP) was 100%, and the selectivity of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) was 99.9%.

[0105] The 1-Cu-Zn / SiO2 catalyst was loaded into the No. 2 packed bed reactor of the second step hydrogenation process. The catalyst was activated in pure hydrogen before use. The activation conditions were: pressure of 0.1 MPa, gas space velocity of 1000 h -1 , the activation temperature is 300℃, the heating rate is 2℃ / min, and the activation time is 10h. After the activation is completed, the system is adjusted to the specified reaction conditions, and the liquid raw material of 1,4-cyclohexanedicarboxylic acid dioctyl ester (DOTCH) in the first step is pumped in to obtain the target product 1,4-cyclohexanedimethanol (CHDM). The reaction conditions are: temperature is 200℃, pressure is 6.0MPa, and the liquid hourly space velocity of dioctyl terephthalate is 0.6h -1The molar ratio of hydrogen to dioctyl terephthalate is 100:1. The conversion rate of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) is 100%, and the selectivity of the target product 1,4-cyclohexanedimethanol (CHDM) is close to 99%. After two-step hydrogenation of dioctyl terephthalate (DOTP), the trans-cis ratio in the product is measured to be 3.5:1.

[0106] Example 2

[0107] The difference from Example 1 is that in the first step of preparing the benzene ring hydrogenation catalyst, 0.0102 g of palladium chloride is weighed in the preparation process of the chloropalladium acid impregnation solution; in the second step of preparing the ester hydrogenation catalyst, 2.2 g of Cu(NO3) is weighed in the preparation process of the uniform solution. 2· 3H2O, 0.5g Zn(NO3) 2· 6H2O. The other steps and process conditions are the same as those in Example 1. 2-Cu-Zn / SiO2 catalyst samples and 2-Cu-Zn / SiO2 catalyst samples are obtained.

[0108] The results are as follows: in the first step of hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol, the conversion of dioctyl terephthalate (DOTP) is 98.5%, and the selectivity of 1,4-cyclohexanedicarboxylic acid dioctyl ester (DOTCH) is 98.9%; in the second step of hydrogenation, the conversion of 1,4-cyclohexanedicarboxylic acid dioctyl ester (DOTCH) is 100%, the selectivity of the target product 1,4-cyclohexanedimethanol (CHDM) is close to 99%, and the trans-cis ratio in the product is 3.5:1.

[0109] Example 3

[0110] The difference from Example 1 is that in the first step of preparing the benzene ring hydrogenation catalyst, 0.0052g of palladium chloride is weighed in the preparation process of the chloropalladium acid impregnation solution; in the second step of preparing the ester hydrogenation catalyst, 2.0g of Cu(NO3)2·3H2O and 0.8g of Zn(NO3)2·6H2O are weighed in the preparation process of the uniform solution. The other steps and process conditions are the same as those in Example 1, and 3-Cu-Zn / SiO2 catalyst samples and 3-Cu-Zn / SiO2 catalyst samples are obtained.

[0111] The results are as follows: in the first step of hydrogenation of dioctyl terephthalate to prepare 1,4-cyclohexanedimethanol by two-step hydrogenation of dioctyl terephthalate, the conversion rate of dioctyl terephthalate (DOTP) is 78.8%, and the selectivity of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) is 98.6%; in the second step of hydrogenation, the conversion rate of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) is 95%, and the selectivity of the target product 1,4-cyclohexanedimethanol (CHDM) is close to 96.8%, and the trans-cis ratio in the product is 3.0:1.

[0112] Example 4

[0113] Catalyst stability test in two-step hydrogenation of dioctyl terephthalate to 1,4-cyclohexanedimethanol:

[0114] The 1-Cu-Zn / SiO2 catalyst sample and the 1-Cu-Zn / SiO2 catalyst sample obtained in Example 1 were subjected to a 1500-hour life test using the same steps and process conditions as in Example 1. The results are shown in the attached figure. Figure 3 , 4 As shown, during the 1500-hour stability test experiment, the conversion rate and selectivity of dioctyl terephthalate (DOTP) and dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) remained basically unchanged, and both the benzene ring hydrogenation catalyst in the first stage and the ester hydrogenation catalyst in the second stage showed excellent stability without any deactivation.

[0115] Comparative Example 1

[0116] The commercial Pd / Al2O3 benzene ring hydrogenation catalyst and Cu-Zn / Al2O3 ester hydrogenation catalyst were loaded into the corresponding No. 1 and No. 2 packed bed reactors, respectively. The other steps and process conditions were the same as those in Example 1. Results In the first step of benzene ring hydrogenation reaction, the conversion rate of dioctyl terephthalate (DOTP) was 90%, and the selectivity of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) was 98.6%. In the second step of ester hydrogenation reaction, the conversion rate of dioctyl 1,4-cyclohexanedicarboxylate (DOTCH) was 85%, the selectivity of the target product 1,4-cyclohexanedimethanol (CHDM) was close to 76.8%, and the trans-cis ratio in the product was 1.3:1.

[0117] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A hydrogenation catalyst system for synthesizing 1,4-cyclohexanedimethanol by a two-step hydrogenation process using dioctyl terephthalate as a raw material, characterized in that: The hydrogenation catalyst system includes a Pd / NiO-Al2O3 catalyst and a Cu-Zn / SiO2 catalyst; In the Pd / NiO-Al2O3 catalyst, single-atom Pd is loaded on the NiO-Al2O3 composite oxide; The Pd / NiO-Al2O3 catalyst has a mesoporous structure; In the Cu-Zn / SiO2 catalyst, Cu and Zn nanoparticles are loaded on SiO2; The Cu-Zn / SiO2 catalyst is a hollow eggshell structure; The hydrogenation catalyst system is obtained by a preparation method comprising the following steps: S1, impregnating NiO-Al2O3 in an impregnation solution containing a palladium source, and drying to obtain a Pd / NiO-Al2O3 catalyst; S2, adding nano silicon oxide balls to a mixed solution containing a copper source and a zinc source and placing the mixed solution in a sealed container, reacting, and calcining I to obtain a Cu-Zn / SiO2 catalyst; In the step S1, the NiO-Al2O3 is prepared by the following preparation method: nickel nitrate is added to a raw material solution containing polyethylene glycol, P123, and anhydrous ethanol to obtain solution a, solution b containing aluminum isopropoxide, concentrated nitric acid, and anhydrous ethanol is added to solution a, heating for reaction, and roasting II to obtain NiO-Al2O3; The P123 is a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

2. The hydrogenation catalyst system according to claim 1, characterized in that In the Pd / NiO-Al2O3 catalyst, the content of the single-atom Pd is 0.1-2.0wt%; In the Cu-Zn / SiO2 catalyst, the content of Cu is 10-50wt%, and the content of Zn is 1-10wt%.

3. The method for preparing the hydrogenation catalyst system according to any one of claims 1 to 2, characterized in that: The steps include: S1, impregnating NiO-Al2O3 in an impregnation solution containing a palladium source, and drying to obtain a Pd / NiO-Al2O3 catalyst; S2. Add nano-silicon oxide balls into a mixed solution containing a copper source and a zinc source and place the mixture in a sealed container for reaction and calcination to obtain a Cu-Zn / SiO2 catalyst.

4. The preparation method according to claim 3, characterized in that: In the step S1, the NiO-Al2O3 is prepared by the following preparation method: nickel nitrate is added to a raw material solution containing polyethylene glycol, P123, and anhydrous ethanol to obtain solution a, solution b containing aluminum isopropoxide, concentrated nitric acid, and anhydrous ethanol is added to solution a, heating for reaction, and roasting II to obtain NiO-Al2O3; The P123 is a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

5. The preparation method according to claim 4, characterized in that: In the preparation method of NiO-Al2O3, the mass concentration of polyethylene glycol in the raw material solution a is 0.05-2.0 g / ml, and the mass concentration of P123 is 0.01-0.1 g / ml.

6. The preparation method according to claim 4, characterized in that: In the preparation method of NiO-Al2O3, the mass concentration of aluminum isopropoxide in the solution b is 0.05-2.0 g / ml, and the mass concentration of nitric acid is 0.05-1.0 g / ml.

7. The preparation method according to claim 4, characterized in that: In the preparation method of NiO-Al2O3, the reaction conditions are: reaction temperature is 40-70°C, and reaction time is 24-60h.

8. The preparation method according to claim 4, characterized in that: In the preparation method of NiO-Al2O3, the calcination conditions II are: calcination at 400-750°C for 4-10 hours.

9. The preparation method according to claim 3, characterized in that: In the step S1, the impregnation solution containing the palladium source further comprises concentrated hydrochloric acid and water.

10. The preparation method according to claim 8, characterized in that: The weight ratio of concentrated hydrochloric acid, water and palladium source in the impregnation solution containing palladium source is (1-4):(100-750):

1.

11. The preparation method according to claim 3, characterized in that: In the step S1, the palladium source is selected from at least one of palladium chloride, palladium nitrate, and palladium acetate.

12. The preparation method according to claim 3, characterized in that: In the step S1, the immersion time is 8 to 36 hours.

13. The preparation method according to claim 3, characterized in that: In step S1, the drying condition is: drying at 70-120° C. for 10-24 hours.

14. The preparation method according to claim 3, characterized in that: In step S2, the copper source is selected from at least one of copper nitrate, copper chloride, and basic copper carbonate; and the zinc source is selected from at least one of zinc nitrate, zinc chloride, and zinc acetate.

15. The preparation method according to claim 3, characterized in that: In step S2, the mixed solution further includes ammonia water and water.

16. The preparation method according to claim 15, characterized in that: The weight ratio of the ammonia water, water to the copper source and zinc source in the mixed solution is (10-100):(300-1000):(2-12):

1.

17. The preparation method according to claim 3, characterized in that: In the step S2, the weight ratio of the nano silicon oxide spheres to the mixed solution is 1:100-400.

18. The preparation method according to claim 4, characterized in that: In step S2, the conditions of the heating reaction are: reaction temperature is 140-180° C., and reaction time is 4-18 hours.

19. The preparation method according to claim 3, characterized in that: In the step S2, the conditions of the calcination I are: calcination at 350-550° C. for 4-10 hours.

20. Use of at least one of the hydrogenation catalyst system according to any one of claims 1 to 2 and the hydrogenation catalyst system prepared according to the preparation method according to any one of claims 3 to 19 in the two-step hydrogenation of dioctyl terephthalate to produce 1,4-cyclohexanedimethanol.

21. The use according to claim 20, characterized in that The steps include: Step 1), contacting dioctyl terephthalate with a Pd / NiO-Al2O3 catalyst, heating for reaction, and obtaining a raw material containing dioctyl 1,4-cyclohexanedicarboxylate; Step 2), the raw material containing dioctyl 1,4-cyclohexanedicarboxylate obtained in step 1) is contacted with a Cu-Zn / SiO2 catalyst, heated for reaction, and 1,4-cyclohexanedimethanol is obtained.

22. The use according to claim 21, characterized in that The step 1) and the step 2) also include activating the Pd / NiO-Al2O3 catalyst and the Cu-Zn / SiO2 catalyst in a hydrogen atmosphere or a mixed atmosphere of hydrogen and inert gas.

23. The use according to claim 22, characterized in that The activation conditions of the Pd / NiO-Al2O3 catalyst are: reaction pressure of 0.05-0.3MPa, gas space velocity of 30-1500h -1 The activation temperature is 200-350°C, the heating rate is 0.5-5°C / min, and the activation time is 2-18h.

24. The use according to claim 22, characterized in that The activation conditions of the Cu-Zn / SiO2 catalyst are: reaction pressure of 0.05-0.3 MPa, gas space velocity of 100-2000 h -1 The activation temperature is 180-350°C, the heating rate is 0.5-10°C / min, and the activation time is 3-38h.

25. The use according to claim 21, characterized in that In the step 1), the conditions of the heating reaction are: the reaction temperature is 130-220°C, the reaction pressure is 2.0-8.0 MPa, and the liquid hourly space velocity of dioctyl terephthalate is 0.01-3.5 h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 5 to 50:

1.

26. The use according to claim 21, characterized in that In the step 2), the conditions of the heating reaction are: the reaction temperature is 200-260°C, the reaction pressure is 2.0-8.0 MPa, and the liquid hourly space velocity of dioctyl terephthalate is 0.01-2.0 h -1 , the molar ratio of hydrogen to dioctyl terephthalate is 50-1000:1.

Citation Information

Patent Citations

  • Method for synthesizing 1,4-cyclohexanedimethanol

    CN102795965A

  • A process for the production of cyclohexanedimethanol

    CN1060153C

  • Low pressure process for the hydrogenation of dimethyl benzenedicarboxylates to the corresponding dimethyl cyclohexanedicarboxylates

    CN1099745A

  • Method used for producing 1, 4-cyclohexanedimethanol

    CN110437033A

  • Catalyst for producing 1,2-cyclohexane dicarboxylic acid diesters

    CN101406840A