A catalyst for polymerization of low carbon olefins and its preparation method and application

By using a low-carbon olefin polymerization catalyst combining ZSM-23 molecular sieve and a Group III transition metal, the problems of low utilization efficiency of ethylene cracking by-product resources and strong catalyst corrosiveness are solved, and high activity and high selectivity olefin polymerization reactions are achieved. Environmental pollution and production costs are reduced.

CN116020542BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111242802.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-10-15
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

In the existing technology, the resource utilization efficiency of C4 and C5 olefins produced by ethylene cracking is low, the catalyst is highly corrosive, product separation is difficult, selectivity is poor, and aluminum trichloride loading efficiency is low, resulting in environmental pollution and low production efficiency.

Method used

ZSM-23 molecular sieve is used as a carrier, combined with Group III transition metals (Fe, Co, Ni) as active components, and a low-carbon olefin polymerization catalyst is prepared through mesoporous structure and hydrothermal treatment for the polymerization of isobutylene or isopentene. Improve catalyst activity and product selectivity.

Benefits of technology

The activity and selectivity of olefin polymerization reaction are improved, environmental pollution is reduced, product separation and catalyst recovery are simplified, and production costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020542B_ABST
    Figure CN116020542B_ABST
Patent Text Reader

Abstract

The present invention discloses a catalyst for polymerization of low-carbon olefins, a preparation method thereof and an application thereof. The catalyst uses a ZSM-23 molecular sieve as a carrier and a transition metal of the first group as an active component. The preparation method of the catalyst comprises the following steps: (1) kneading a mesoporous ZSM-23 molecular sieve, a binder and a peptizing agent, and preparing the catalyst carrier after drying and calcining; (2) introducing an active metal component into the catalyst carrier of step (1), and preparing the catalyst after drying and calcining. The catalyst is used for polymerization of low-carbon olefins, such as polymerization of isobutylene and / or isopentene, and has the advantages of high activity, easy separation of products, and reduced environmental pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a low-carbon olefin polymerization catalyst and a preparation method and application thereof, and in particular to a low-carbon olefin polymerization catalyst using a ZSM-23 molecular sieve as a carrier and a preparation method and application thereof. Background Art

[0002] In recent years, with the rapid development of my country's economy, China's ethylene production capacity has grown rapidly, making it the world's second largest ethylene producer after the United States. The C4 and C5 fractions produced as byproducts of ethylene cracking units account for about 40-50wt.% of ethylene production, respectively. The olefin content is more than 50%, and the olefins contained have considerable potential for deep processing. In addition to producing medium and high polyisobutylene, they can also produce high value-added isoparaffin solvent oil through oligomerization and hydrogenation. Therefore, how to reasonably utilize the C4 and C5 olefin resources produced as byproducts of ethylene cracking has gradually attracted people's attention, which is of great significance to petrochemical enterprises in tapping potential and increasing efficiency and developing fine chemicals.

[0003] At present, polyisobutylene usually uses anhydrous aluminum chloride as a catalyst. Anhydrous aluminum chloride is dissolved in hydrocarbons and mixed with isobutylene for homogeneous reaction. This homogeneous reaction usually uses a traditional stirred tank reactor. When the reaction is about to start, the catalyst and the raw materials are not evenly mixed, which will cause isobutylene to react violently with the area with high catalyst concentration, and the reaction heat cannot be diffused and temperature rises. There are problems such as low product yield, wide product distribution, and poor selectivity. This homogeneous method also has low production efficiency and difficulty in product separation. At the same time, aluminum chloride is highly corrosive, polluting the environment and corroding equipment.

[0004] Immobilized catalyst systems have been a research hotspot in the chemical industry in recent years. By combining catalytic functional components with ideal catalyst carriers to form immobilized catalysts, the activity of the catalyst can be maintained and it can also be easily separated from the reaction products and recycled, which greatly reduces the consumption of catalysts and post-treatment processes and the emission of "three wastes". While being more environmentally friendly, it can also save a lot of costs. Therefore, the development of new environmentally friendly immobilized catalysts for olefin polymerization has attracted much attention in recent years.

[0005] USP4929800 uses CCl4, CH3Cl or CH2Cl2 as solvents, dissolves aluminum chloride in them, and then adds carriers such as silicon oxide or aluminum oxide, and refluxes for several hours or days at 50~80℃ under N2 protection conditions to obtain olefin polymerization catalysts. This method is relatively simple using a solution method, but due to the low solubility of the solvent in aluminum chloride, and the loading degree of aluminum chloride depends on the pore structure and size of the carrier. Therefore, this method has low aluminum chloride loading efficiency and low polymerization reaction activity, and also causes waste of aluminum chloride raw materials and pollutes the environment.

[0006] CN107185560A relates to a method for preparing a supported oxide catalyst. The method mainly uses macroporous alumina as a carrier, and supports iron sulfate and nickel sulfate to prepare a finished catalyst. The catalyst requires mild reaction conditions, but the method has problems such as different molecular chain lengths of the polymerized product, wide product distribution, and low selectivity.

[0007] CN102240563 discloses an olefin polymerization catalyst with Al2O3 as a carrier and AlCl3 and a Group VIII transition metal salt as active components. The catalyst is used to catalyze the polymerization reaction of 1-decene or 1-octene, overcoming the problems of strong corrosiveness of aluminum chloride and difficulty in product separation. However, the catalyst has the problems of low catalytic activity and poor stability.

[0008] ZSM-23 molecular sieve is a molecular sieve material with a high silicon-aluminum ratio and an MTT topological structure. Its one-dimensional teardrop-shaped pores are composed of ten-membered rings. With its unique pore structure and adjustable acid properties, ZSM-23 molecular sieves are widely used in the fields of separation, adsorption and catalysis, playing an irreplaceable role. However, ZSM-23 is a microporous molecular sieve, and its ability to process the conversion of larger molecules is limited by the pore size. Therefore, in order to further expand its application range, it is of great significance to prepare mesoporous ZSM-23 molecular sieves with excellent performance. Summary of the invention

[0009] In order to overcome the deficiencies in the prior art, the present invention provides a catalyst for polymerization of low-carbon olefins, a preparation method thereof and an application thereof. The catalyst is used for polymerization of low-carbon olefins such as isobutylene and / or isopentene and has the advantages of high activity, easy separation of products, reduced environmental pollution, etc.

[0010] A catalyst for polymerization of low-carbon olefins, the catalyst using ZSM-23 molecular sieve as a carrier, The transition metal of the first group is an active component, and the content of ZSM-23 molecular sieve is 30wt% to 80wt%, preferably 50wt% to 70wt%, based on the weight of the final low-carbon olefin polymerization catalyst. The content of the transition metal oxide of the group A is 1wt%~35wt%, preferably 2wt%~10wt%; the specific surface area of ​​the catalyst is 300-430m 2 / g, pore volume is 0.31-0.5cm 3 / g, micropore specific surface area is 50-170m 2 / g, mesoporous specific surface area is 150-310m 2 / g; preferably, the specific surface area is 320-405m 2 / g, pore volume is 0.34-0.45cm 3 / g, micropore specific surface area is 80-140m2 / g, mesopore specific surface area is 181-295m 2 / g.

[0011] In the catalyst for polymerization of light olefins of the present invention, the The transition metal is one or more of Fe, Co, or Ni.

[0012] In the low-carbon olefin polymerization catalyst of the present invention, the mesopore volume of the ZSM-23 molecular sieve with a pore size of 3-8 nm, preferably 3-6 nm, accounts for 45-90% of the total pore volume of the molecular sieve, preferably 50-85%, and more preferably 55-81%.

[0013] In the low-carbon olefin polymerization catalyst of the present invention, the relative crystallinity of the molecular sieve is 95-120%, and the relative crystallinity retention of the molecular sieve after hydrothermal treatment with 600°C steam for 2 hours is 95-100%.

[0014] A method for preparing a low-carbon olefin polymerization catalyst, characterized in that it comprises the following steps:

[0015] (1) The mesoporous ZSM-23 molecular sieve, the binder and the peptizing agent are kneaded and formed into a catalyst carrier after drying and calcining;

[0016] (2) Step (1) An active metal component is introduced onto the catalyst carrier, which is dried and calcined to prepare a catalyst.

[0017] In step (1) of the method of the present invention, the mesoporous ZSM-23 molecular sieve has a pore size of 3-8 nm, preferably 3-6 nm, and the mesopore volume accounts for 45-90%, preferably 50-85%, and more preferably 55-81% of the total pore volume of the molecular sieve.

[0018] In step (1) of the method of the present invention, the relative crystallinity of the mesoporous ZSM-23 molecular sieve is 95-120%, and the relative crystallinity retention of the molecular sieve after hydrothermal treatment with water vapor at 600° C. for 2 hours is 95-100%.

[0019] In step (1) of the method of the present invention, the binder used can be small-pore alumina, and the pore volume of the small-pore alumina used is 0.3-0.5 ml / g, and the specific surface area is 200-400 m 2 / g. The peptizing agent used can be one or more of aluminum sulfate, citric acid, nitric acid, acetic acid, oxalic acid, etc.

[0020] In step (1) of the method of the present invention, the mesoporous ZSM-23 molecular sieve, small pore alumina and peptizing agent are mechanically mixed and formed, and then dried at a temperature of 80-150° C. for 2-10 hours and calcined at 500-600° C. for 3-6 hours to prepare a catalyst carrier. The catalyst carrier can be formed according to actual needs and the shape can be cylindrical, clover, etc.

[0021] In step (2) of the method of the present invention, the active metal component can be introduced by impregnation, either by equal volume impregnation or by excess volume impregnation.

[0022] In step (2) of the method of the present invention, the drying conditions are as follows: the drying temperature is 60°C to 180°C, preferably 90°C to 120°C, and the drying time is 0.5h to 20.0h, preferably 3.0h to 6.0h; the calcination conditions are as follows: the calcination temperature is 200°C to 750°C, preferably 500°C to 650°C, and the calcination time is 0.5h to 20.0h, preferably 3.0h to 6.0h. The drying and calcination can be carried out in an oxygen-containing atmosphere, with no particular limitation on the oxygen concentration, such as an air atmosphere, or in an inert atmosphere, such as a nitrogen atmosphere.

[0023] In step (2) of the method of the present invention, at 20-60°C, the mesoporous ZSM-23 molecular sieve is heated to 0.1-2.0 M The precipitate is soaked in the nitrate of transition metal Fe, Co, or Ni for 1 to 4 hours, then dried at 60 to 120°C for 1 to 6 hours, and then calcined at 200 to 600°C for 4 to 12 hours.

[0024] The application of the above-mentioned low-carbon olefin polymerization catalyst adopts a fixed bed reactor to carry out olefin polymerization reaction with isobutylene or isopentene as raw material; the process conditions are: reaction temperature is 40~120℃, pressure is 1.0~6.0MPa, volume space velocity is 0.6~1.5h -1 .

[0025] Compared with the prior art, the method of the present invention has the following advantages:

[0026] (1) The ZSM-23 molecular sieve synthesized by the method of the present invention has both the acidic properties of the microporous structure that can be adjusted and the macroporous characteristics of the mesoporous structure, which further improves the reaction activity and product selectivity of the olefin polymerization reaction.

[0027] (2) The present invention uses a novel catalyst combining active metal and molecular sieve, which synergistically catalyze each other to further improve the conversion rate of olefin polymerization reaction.

[0028] (3) The present invention solves the problems of corrosion of traditional low-carbon olefin polymerization reaction equipment, high chlorine content of products, and environmental pollution caused by wastewater generated by catalyst post-treatment. The polymerized olefin products are easier to separate and the reaction is easier to control. DETAILED DESCRIPTION

[0029] A mesoporous ZSM-23 molecular sieve in the method of the present invention comprises the following preparation steps:

[0030] a. preparing or selecting amorphous silicon dioxide;

[0031] b. treating amorphous silica with an alkali;

[0032] c ZSM-23 molecular sieve was prepared using alkali-treated amorphous silica as the silicon source.

[0033] In step a of the above method, the amorphous silicon dioxide has a specific surface area of ​​600-1300m 2 / g, preferably 700-1200m 2 / g; pore volume is 0.6-1.3cm 3 / g, preferably 0.7-1.2cm 3 / g; the pore diameter is 1-15nm, preferably 2-10nm.

[0034] In step a of the above method, the amorphous silica preparation process is as follows: adding a silicon source to deionized water and dispersing it evenly, then adding a surfactant and stirring; adjusting the solution pH to 1-5, preferably 1.5-4, and heating it in a water bath for a period of time; filtering, washing, drying, and calcining to obtain amorphous silica.

[0035] In the above method, during the preparation of amorphous silicon dioxide, the silicon source is an inorganic silicon source, preferably one or more of water glass, silica sol or white carbon black.

[0036] In the above method, during the preparation of amorphous silicon dioxide, the surfactant is one or more of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, and octadecyltrimethylammonium bromide.

[0037] In the above method, during the preparation of the amorphous silica, the molar ratio of the silicon source in terms of SiO2 to the surfactant is 1:(0.02-0.3), preferably 1:(0.05-0.2).

[0038] In the above method, during the preparation of the amorphous silicon dioxide, the molar ratio of the silicon source in terms of SiO2 to deionized water is 1:(30-300), preferably 1:(50-220).

[0039] In the above method, during the preparation of the amorphous silica, the heating temperature is 30-80°C, preferably 40-70°C, and the heating time is 0.5-8h, preferably 3-6h.

[0040] In step b of the above method, the alkali treatment is to add the amorphous silicon dioxide prepared in step a into an alkaline solution and heat and stir.

[0041] In the above method, the alkali treatment is carried out with an inorganic alkali, and the inorganic alkali is sodium hydroxide, potassium hydroxide or ammonia water.

[0042] One or more of the .

[0043] In the above method, the alkali treatment heating and stirring time is 0.5-12h, preferably 2-8h; the heating temperature is 25-60°C, preferably 30-50°C.

[0044] In the above method, the molar ratio of amorphous silica calculated as SiO2 to the inorganic base is 0.05-0.24, preferably 0.06-0.22.

[0045] In step c of the above method, in preparing ZSM-23 molecular sieve using alkali-treated amorphous silicon dioxide as a silicon source, any method for preparing ZSM-23 molecular sieve known in the prior art may be used, and a method for preparing ZSM-23 molecular sieve that is not yet known in the prior art but will be known in the future may also be used. For example, a known method is disclosed in U.S. Pat. No. 4,990,342 of Mobil Oil Corporation.

[0046] In step c of the above method, preferably, alkali-treated amorphous silicon dioxide is used as a silicon source, and the silicon source is mixed with an aluminum source, an alkali source (MOH), a template (R), and water to form a gel, and the ZSM-23 molecular sieve is obtained after crystallization, filtration, washing, drying, and calcination;

[0047] More preferably, the molar ratio of silicon source (in terms of SiO2): aluminum source (in terms of Al2O3): alkali source (in terms of hydroxide): template: H2O in the gel is 1: (0.003-0.03): (0.03-0.3): (0.05-2): (10-90); further preferably, the molar ratio of silicon source (in terms of SiO2): aluminum source (in terms of Al2O3): alkali source (in terms of hydroxide): template: H2O in the gel is 1: (0.005-0.02): (0.03-0.16): (0.08-1.6): (20-70);

[0048] More preferably, the gel is crystallized at 150-200°C, preferably 170-180°C, for 24-96h, preferably 36-72h, and then filtered, washed, dried, and calcined to obtain a ZSM-23 molecular sieve; and / or

[0049] More preferably, the drying temperature is 80-120° C., the drying time is 4-12 hours, the roasting temperature is 500-600° C., and the roasting time is 2-6 hours.

[0050] In order to better illustrate the present invention, the following is further described in conjunction with embodiments and comparative examples, but the present invention is not limited to these embodiments.

[0051] The analysis method of the present invention is as follows: The specific surface area and pore volume of the catalyst or molecular sieve are measured by using an ASAP 2405 physical adsorption instrument from Micromeritics, USA, where the specific surface area refers to the sum of the micropore specific surface area and the mesopore specific surface area. The loaded metal content is measured by atomic absorption spectroscopy.

[0052] The XRD spectrum of the sample was obtained by a Dmax2500 X-ray diffractometer produced by Rigaku Corporation of Japan, and the relative crystallinity of the sample was calculated. The sum of the heights of the diffraction peaks at 2θ of about 11.3 and 19.5-23° in the XRD spectrum of conventional ZSM-23 molecular sieve was taken as 100% crystallinity, and the relative crystallinity of other samples was obtained by comparison.

[0053] Embodiment 1:

[0054] (1) Preparation of carrier:

[0055] Add 50g of water glass (SiO2 mass fraction is 27%) to 250g of deionized water, stir and disperse evenly, then add octadecyltrimethylammonium chloride (C18TMACl) and stir for 0.5h, wherein the molar ratio of SiO2 to C18TMACl is 1:0.08; adjust the pH of the solution to 2 with hydrochloric acid, place it in a 50°C water bath and heat it for 4h; after completion, filter, wash, dry at 80°C for 8h, and calcine at 550°C for 3h to obtain amorphous silica;

[0056] Dissolve 0.35 g of NaOH in 35 mL of deionized water, add 3.7 g of the prepared mesoporous silicon source, and stir in a 45 °C water bath for 3 h;

[0057] After aluminum sulfate and isopropylamine (IPA) are dissolved in the remaining water in sequence, the silicon source dispersion obtained in a) is added thereto to obtain a gel with a total molar ratio of SiO2 in the silicon source: Al2O3 in the aluminum source: OH-: IPA: H2O = 1: 0.01: 0.08: 1.0: 50. After crystallization at 180°C for 48 hours, the ZSM-23 molecular sieve is obtained after filtration, washing, drying and calcination. The properties of the ZSM-23 molecular sieve are as follows: the molecular sieve has a specific surface area of ​​395 m 2 / g, pore volume is 0.42cm 3 / g, micropore specific surface area is 105m 2 / g, mesopore specific surface area is 290m 2 / g, the mesopore content with a pore size of 3-8nm is 77%, the relative crystallinity is 102%, and the relative crystallinity after hydrothermal treatment is 103%.

[0058] The ZSM-23 molecular sieve, small pore alumina and binder were mechanically mixed and formed, and then dried at 120°C for 8 hours and calcined at 600°C for 4 hours to prepare a catalyst carrier. The small pore alumina used has a pore volume of 0.5 ml / g and a specific surface area of ​​300 m 2 / g.

[0059] (2) Preparation of catalyst:

[0060] 300 g of the carrier was added to 1.0 M ferric nitrate solution, stirred evenly, soaked at 30°C for 3 hours, and then vacuum dried at 70°C for 3 hours. Then, it was calcined at 500°C for 8 hours.

[0061] Through analysis and characterization, the specific surface area of ​​the catalyst is 305m 2 / g, pore volume is 0.43cm 3 / g, micropore specific surface area is 75m 2 / g, mesopore specific surface area is 230m 2 / g. The iron oxide content in the catalyst is 3.55 wt%, and the mass content of ZSM-23 molecular sieve is 67.5%.

[0062] (3) Olefin polymerization reaction:

[0063] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor with a catalyst loading volume of 40 ml and a volumetric space velocity of 1.0 h -1 , the reaction temperature is 80°C, the pressure is 4.0MPa, and the product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0064] Embodiment 2:

[0065] 300 g of the carrier in Example 1 was added to a 0.5 M ferric nitrate solution, stirred evenly, soaked at 30° C. for 5 h, and then vacuum dried at 70° C. for 3 h, and then calcined at 500° C. for 8 h.

[0066] Through analysis and characterization, the specific surface area of ​​the catalyst is 316m 2 / g, pore volume is 0.42cm 3 / g, micropore specific surface area is 78m 2 / g, mesopore specific surface area is 238m 2 / g. The iron oxide content in the catalyst is 2.31 wt%, and the mass content of ZSM-23 molecular sieve is 68.2%.

[0067] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor. The reaction conditions were the same as those in Example 1. The product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0068] Embodiment 3:

[0069] 300 g of the carrier in Example 1 was added to a 1.5 M ferric nitrate solution, stirred evenly, soaked at 30° C. for 5 h, and then vacuum dried at 70° C. for 3 h, and then calcined at 500° C. for 8 h.

[0070] Through analysis and characterization, the specific surface area of ​​the catalyst is 295m 2 / g, pore volume is 0.42cm 3 / g, micropore specific surface area is 78m 2 / g, mesopore specific surface area is 238m 2 / g. The iron oxide content in the catalyst is 5.26 wt%, and the mass content of ZSM-23 molecular sieve is 66.2%.

[0071] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor. The reaction conditions were the same as those in Example 1. The product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0072] Embodiment 4:

[0073] 300 g of the carrier in Example 1 was added to a 1.0 M nickel nitrate solution, stirred evenly, soaked at 30° C. for 6 h, and then vacuum dried at 80° C. for 3 h, and then calcined at 500° C. for 8 h.

[0074] Through analysis and characterization, the specific surface area of ​​the catalyst is 303m 2 / g, pore volume is 0.43cm 3 / g, micropore specific surface area is 73m 2 / g, mesopore specific surface area is 230m 2 / g. The nickel oxide content in the catalyst is 2.32 wt%.

[0075] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor. The reaction conditions were the same as those in Example 1. The product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0076] Comparative Example 1:

[0077] (1) Preparation of molecular sieves:

[0078] Water glass, aluminum sulfate, isopropylamine (IPA), sodium hydroxide and water were mixed to prepare a gel with a total molar ratio of SiO2 in silicon source: Al2O3 in aluminum source: NaOH: IPA: H2O = 1:0.01:0.08:1.0:50. After heating at 180°C for 72h, the conventional ZSM-23 molecular sieve was obtained after filtering, washing, drying and calcining. The properties of the molecular sieve are as follows: The specific surface area of ​​the molecular sieve is 228m 2 / g, pore volume is 0.24cm 3 / g, micropore specific surface area is 188m 2 / g, mesopore specific surface area is 40m 2 / g, the mesopore content with a pore size of 3-8nm is 18%, the relative crystallinity is 100%, and the relative crystallinity after hydrothermal treatment is 101%.

[0079] Conventional ZSM-23 molecular sieve, small pore alumina and binder were mechanically mixed and formed, then dried at 120°C for 8 hours and calcined at 600°C for 4 hours to prepare a catalyst carrier. The small pore alumina used had a pore volume of 0.5 ml / g and a specific surface area of ​​300 m 2 / g.

[0080] (2) Preparation of Catalyst

[0081] 300 g of the carrier was added to 1.0 M ferric nitrate solution, stirred evenly, soaked at 30°C for 3 hours, and then vacuum dried at 70°C for 3 hours. Then, it was calcined at 500°C for 8 hours.

[0082] Through analytical characterization, the specific surface area of ​​the catalyst is 168m 2 / g, pore volume is 0.26cm 3 / g, micropore specific surface area is 132m 2 / g, mesopore specific surface area is 36m 2 / g. The iron oxide content in the catalyst is 2.03 wt%, and the mass content of ZSM-23 molecular sieve is 69.1%.

[0083] (3) Olefin polymerization

[0084] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor. The reaction conditions were the same as those in Example 1. The product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0085] Comparative Example 2:

[0086] The catalyst was prepared according to the method of Example 1 of CN107185560A, and the catalyst contained 5.0 wt% of iron sulfate, 2.5 wt% of nickel sulfate and 92.5 wt% of an alumina carrier having a macroporous structure.

[0087] Using isobutylene as raw material, polymerization reaction was carried out in a small fixed bed reactor. The reaction conditions were the same as those in Example 1. The product distillation range distribution and isobutylene conversion rate are shown in Table 1.

[0088] <160℃Product yield, % 160℃~340℃ product yield, % >340℃Product yield, % Conversion rate, % Example 1 14.5 79.2 10.3 92.9 Example 2 18.8 75.2 6.0 91.5 Example 3 9.7 77.8 12.5 95.2 Example 4 14.7 74.4 0.9 90.1 Comparative Example 1 56.2 38.0 5.8 63.2 Comparative Example 2 43.7 26.8 29.5 87.5

Claims

1. A catalyst for the polymerization of light olefins, characterized in that: The catalyst is supported by ZSM-23 molecular sieve. The transition metal of the first group is the active component, and the content of ZSM-23 molecular sieve is 30wt%~80wt% based on the weight of the final low-carbon olefin polymerization catalyst. The content of the transition metal oxide of the group A is 1wt%~35wt%; the specific surface area of ​​the catalyst is 300-430m 2 / g, pore volume is 0.31-0.5cm 3 / g, micropore specific surface area is 50-170m 2 / g, mesoporous specific surface area is 150-310m 2 / g; The mesopore volume of the ZSM-23 molecular sieve with a pore size of 3-8 nm accounts for 45-90% of the total pore volume of the molecular sieve; The low carbon olefin is isobutylene or isopentene; The said The transition metal of group A is one or more of Fe, Co, or Ni; The ZSM-23 molecular sieve is prepared by using alkali-treated amorphous silicon dioxide as a silicon source.

2. The catalyst according to claim 1, characterized in that: Based on the weight of the final low-carbon olefin polymerization catalyst, the content of ZSM-23 molecular sieve is 50wt%~70wt%, The content of the transition metal oxide of the group A is 2wt%~10wt%; the specific surface area of ​​the catalyst is 320-405m 2 / g, pore volume is 0.34-0.45cm 3 / g, micropore specific surface area is 80-140m 2 / g, mesopore specific surface area is 181-295m 2 / g.

3. The catalyst according to claim 1, characterized in that: The mesopore volume of the ZSM-23 molecular sieve with a pore size of 3-8 nm accounts for 50-85% of the total pore volume of the molecular sieve.

4. The catalyst according to claim 1, characterized in that: The pore size of the ZSM-23 molecular sieve is 3-8 nm, and the mesopore volume accounts for 55-81% of the total pore volume of the molecular sieve.

5. The catalyst according to claim 1, characterized in that: The relative crystallinity of the molecular sieve is 95-120%, and the relative crystallinity retention of the molecular sieve after hydrothermal treatment with 600° C. steam for 2 hours is 95-100%.

6. The method for preparing the catalyst according to any one of claims 1 to 5, characterized in that: The steps include: (1) The mesoporous ZSM-23 molecular sieve, the binder and the peptizing agent are kneaded and formed into a catalyst carrier after drying and calcining; (2) Step (1) An active metal component is introduced onto a catalyst carrier, which is dried and calcined to prepare a catalyst.

7. The method according to claim 6, characterized in that: In step (1), the binder used is small-pore alumina, the pore volume of the small-pore alumina used is 0.3-0.5 ml / g, and the specific surface area is 200-400 m 2 / g.

8. The method according to claim 6, characterized in that: In step (1), the peptizing agent used is one or more of aluminum sulfate, citric acid, nitric acid, acetic acid, and oxalic acid.

9. The method according to claim 6, characterized in that: In step (1), the mesoporous ZSM-23 molecular sieve, small pore alumina and peptizing agent are mechanically mixed and formed, and then dried at a temperature of 80-150° C. for 2-10 hours and calcined at 500-600° C. for 3-6 hours to prepare a catalyst carrier.

10. The method according to claim 6, characterized in that: In step (2), the active metal component is introduced by impregnation, either equal volume impregnation or excess volume impregnation.

11. The method according to claim 6, characterized in that: In step (2), the drying conditions are as follows: the drying temperature is 60°C to 180°C, and the drying time is 0.5h to 20.0h; the roasting conditions are as follows: the roasting temperature is 200°C to 750°C, and the roasting time is 0.5h to 20.0h.

12. The method according to claim 11, characterized in that: In step (2), the drying temperature is 90°C to 120°C.

13. The method according to claim 11, characterized in that: In step (2), the drying time is 3.0 h to 6.0 h.

14. The method according to claim 11, characterized in that: In step (2), the calcination temperature is 500°C to 650°C.

15. The method according to claim 11, characterized in that: In step (2), the calcination time is 3.0 h to 6.0 h.

16. The method according to claim 6, characterized in that: In step (2), at 20-60°C, the mesoporous ZSM-23 molecular sieve is heated to 0.1-2.0 M. The obtained alloy is immersed in the nitrate of transition metal Fe, Co, or Ni for 1 to 4 hours, then dried at 60 to 120°C for 1 to 6 hours, and then calcined at 200 to 600°C for 4 to 12 hours.

17. Use of a catalyst according to any one of claims 1 to 5, characterized in that: A fixed bed reactor is used to carry out olefin polymerization reaction with isobutylene or isopentene as raw material.

18. The use according to claim 17, characterized in that: The process conditions are: reaction temperature 40~120℃, pressure 1.0~6.0MPa, volume space velocity 0.6~1.5h -1 .