Lithium iron phosphate positive electrode material and preparation method and application thereof

By using Fe-MOF material as the iron source, combined with sintering treatment and inorganic-organic component characteristics, the problem of poor conductivity and large particle size difference of lithium iron phosphate cathode material is solved, and the conductivity and particle uniformity are improved, which is suitable for Mass production and improved performance of lithium-ion batteries.

CN116022762BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211650234.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-22
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The lithium iron phosphate cathode material has poor conductivity and large particle size differences, resulting in poor electrical performance. Existing modification methods such as ion doping or carbon coating have problems with uneven doping or uneven coating.

Method used

Fe-MOF material is used as the iron source, mixed, ground and sintered in a protective atmosphere. Combined with the inorganic-organic component characteristics of Fe-MOF material, the synthesis and coating process is simplified, the elements are evenly dispersed and evenly coated, and the conductivity is improved. properties and particle uniformity.

Benefits of technology

It effectively improves the conductivity and particle uniformity of the lithium iron phosphate cathode material, simplifies the process steps, is suitable for large-scale production, and shows good stability and rate performance in lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116022762B_ABST
    Figure CN116022762B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-ion battery positive electrode materials, and in particular to a lithium iron phosphate positive electrode material and a preparation method and application thereof. The preparation method of the lithium iron phosphate positive electrode material comprises the following steps: after the iron source, phosphorus source and lithium source are mixed and ground, sintering treatment is carried out under a protective atmosphere; the iron source comprises a Fe-MOF material. The present invention utilizes the rich porosity and unique hierarchical porous structure of MOFs materials, and uses them as templates to prepare MOFs-based lithium iron phosphate positive electrode materials, which can achieve the effects of grain refinement, ensuring particle uniformity, and improving electrical conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are mainly composed of positive electrode, negative electrode, electrolyte, separator and other parts. Among them, the performance improvement of positive electrode materials is particularly important. A large number of scientific researchers are working hard to improve the performance of positive electrode materials and develop new positive electrode materials. Among many positive electrode materials, lithium iron phosphate positive electrode materials have attracted widespread attention and development due to their good stability, high safety, low cost, non-toxic and environmentally friendly characteristics. In recent years, metal organic framework materials (MOFs) have attracted widespread attention as a new type of material. They are mainly composed of metal ions as the center and organic ligands as the skeleton, and have diverse and flexible design and regulation characteristics.

[0003] At present, the preparation method of lithium iron phosphate positive electrode material has gradually matured. In industrial production, high-temperature solid-phase method is generally used for synthesis and preparation. This method is low-cost but easily leads to problems such as powder agglomeration and serious powder agglomeration effect, which is not conducive to the full play of electrical performance. In addition, in order to improve the poor conductivity of lithium iron phosphate positive electrode materials, ion doping or carbon coating is required during the modification. Although these methods can effectively improve the conductivity problem, they are also prone to problems such as uneven doping or uneven coating, affecting the microstructure and particle size distribution of the material and ultimately leading to poor electrical performance.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a method for preparing a lithium iron phosphate positive electrode material to solve the technical problems existing in the prior art such as poor conductivity and large particle size differences of the lithium iron phosphate positive electrode material.

[0006] Another object of the present invention is to provide a lithium iron phosphate positive electrode material prepared by the above preparation method.

[0007] Another object of the present invention is to provide a lithium ion battery.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A method for preparing a lithium iron phosphate positive electrode material comprises the following steps:

[0010] The iron source, phosphorus source and lithium source are mixed and ground, and then sintered under a protective atmosphere;

[0011] The iron source includes a Fe-MOF material.

[0012] In a specific embodiment of the present invention, the molar ratio of the iron source, the phosphorus source and the lithium source in terms of Fe, P and Li is (1-2):(0.8-1.2):1.

[0013] In a specific embodiment of the present invention, the phosphorus source includes any one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate and lithium dihydrogen phosphate; the lithium source includes any one or more of lithium carbonate, lithium hydroxide, lithium oxalate and lithium dihydrogen phosphate.

[0014] In a specific embodiment of the present invention, the grinding is ball milling. Further, the ball milling time is 4 to 12 hours and the rotation speed of the ball mill is 1000 to 4000 rpm.

[0015] In a specific embodiment of the present invention, the protective atmosphere includes argon and / or nitrogen.

[0016] In a specific embodiment of the present invention, the temperature of the sintering treatment is 700-800° C.; the holding time of the sintering treatment is 9-12 hours.

[0017] In a specific embodiment of the present invention, the preparation of the Fe-MOF material includes: dispersing iron salt in a solution of an organic ligand, heating the solution at 140-180° C. for 6-12 hours, cooling the solution to room temperature, washing and drying the solution.

[0018] In a specific embodiment of the present invention, the molar ratio of the iron salt to the organic ligand is 1:(0.5-2).

[0019] In a specific embodiment of the present invention, the iron salt includes any one or more of ferric chloride, ferric nitrate and ferric sulfate.

[0020] In a specific embodiment of the present invention, the solution of the organic ligand is prepared by mixing the organic ligand and a solvent. Further, the solvent includes at least one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).

[0021] In a specific embodiment of the present invention, in the Fe-MOF material, the organic ligands constituting the organic skeleton include at least one polycarboxylic acid organic ligand; the number of carboxylic acid groups in a single polycarboxylic acid organic ligand is ≥3.

[0022] In a specific embodiment of the present invention, in the Fe-MOF material, the organic ligand constituting the organic framework includes trimesic acid.

[0023] In a specific embodiment of the present invention, the process further comprises: cooling the sintered material, and then grinding and screening it.

[0024] The present invention also provides a lithium iron phosphate positive electrode material prepared by using any one of the above-mentioned methods for preparing the lithium iron phosphate positive electrode material.

[0025] In a specific embodiment of the present invention, the average particle size of the lithium iron phosphate positive electrode material is 1.12-2.01 μm.

[0026] In a specific embodiment of the present invention, the particle size concentration of the lithium iron phosphate positive electrode material is (D90-D10) / D50 is 2.56 to 4.26.

[0027] In a specific embodiment of the present invention, the powder resistivity of the lithium iron phosphate positive electrode material is 19.54 to 65.45 Ohm-cm under a pressure of 4 kN.

[0028] The present invention also provides a lithium-ion battery, comprising any one of the above-mentioned lithium iron phosphate positive electrode materials.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The present invention uses Fe-MOF as the iron source. On the one hand, it can make the elements evenly dispersed and weaken the agglomeration effect; on the other hand, the metal element Fe is "anchored" on the organic ligand. After high-temperature calcination, the organic ligand can be carbonized and evenly coated on the positive electrode material as a carbon source, ensuring the uniformity of the coating and thereby improving the conductivity of the material.

[0031] (2) The present invention utilizes the characteristics of Fe-MOF materials that have both organic and inorganic components, and combines the synthesis and coating processes of lithium iron phosphate positive electrode materials into one, thereby simplifying the process steps and being suitable for large-scale production.

[0032] (3) The present invention utilizes the rich porosity and unique hierarchical porous structure of MOFs materials and uses them as templates to prepare MOFs-based lithium iron phosphate positive electrode materials, which can achieve the effects of refining grains, ensuring particle uniformity, and improving electrical conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 This is the XRD pattern of the lithium iron phosphate positive electrode material prepared in Example 5 of the present invention;

[0035] Figure 2This is the XRD diagram of the lithium iron phosphate positive electrode material prepared in Comparative Example 1. DETAILED DESCRIPTION

[0036] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] A method for preparing a lithium iron phosphate positive electrode material comprises the following steps:

[0038] The iron source, phosphorus source and lithium source are mixed and ground, and then sintered under a protective atmosphere;

[0039] The iron source includes a Fe-MOF material.

[0040] Among them, Fe-MOF material refers to a material in which the metal central ion is Fe and the organic skeleton of MOF is an organic ligand. Fe-MOF can be used as both an iron source and a carbon source. The Fe element is first "anchored" on the organic ligand. Since the microscopic size of Fe-MOF is at the nanometer level, it can induce the obtained lithium iron phosphate particles to have a smaller particle size; while saving the process of adding an organic carbon source, it is beneficial to improve its conductivity. In addition, it can also effectively avoid problems such as poor particle uniformity caused by insufficient mixing.

[0041] The present invention utilizes the characteristics of Fe-MOF materials that have both inorganic and organic components, combines the two processes of synthesis and coating of lithium iron phosphate positive electrode materials into one, saves the process of adding dispersants and coating agents in batches, simplifies the process steps, and solves the problems of conductivity and particle uniformity, showing good stability and rate performance. In button batteries, the capacity retention rate of 50 cycles at room temperature 1C is improved by about 2%, and the discharge capacity at different rates is improved.

[0042] In a specific embodiment of the present invention, the molar ratio of the iron source, the phosphorus source and the lithium source in terms of Fe, P and Li is (1-2):(0.8-1.2):1.

[0043] For example, in different embodiments, the molar ratio of the iron source, the phosphorus source and the lithium source, calculated as Fe, P and Li, can be exemplified as 1:0.8:1, 1:1:1, 1:1.2:1, 1.5:0.8:1, 2:0.8:1, 1.5:1:1, 2:1:1, 1.5:1.2:1, 2:1.2:1, etc.

[0044] In a specific embodiment of the present invention, the phosphorus source includes any one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate and lithium dihydrogen phosphate; the lithium source includes any one or more of lithium carbonate, lithium hydroxide, lithium oxalate and lithium dihydrogen phosphate.

[0045] The types of phosphorus source and lithium source can be adjusted according to actual needs. When lithium dihydrogen phosphate is used, it serves as both phosphorus source and lithium source.

[0046] In a specific embodiment of the present invention, the grinding is ball milling. Further, the ball milling time is 4 to 12 hours and the rotation speed of the ball mill is 1000 to 4000 rpm.

[0047] For example, in different embodiments, the ball milling time can be exemplified as 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, etc.; the ball milling speed can be exemplified as 1000rpm, 2000rpm, 3000rpm, 4000rpm, etc.

[0048] In actual operation, the ball milling operation can be performed in a high-speed ball mill. By adopting the above ball milling conditions, the iron source, phosphorus source and lithium source are fully mixed.

[0049] In a specific embodiment of the present invention, the protective atmosphere includes argon and / or nitrogen.

[0050] In actual operation, the sintering process can be carried out in a high-temperature tube furnace or other equipment. During sintering, the equipment is filled with a protective atmosphere.

[0051] In a specific embodiment of the present invention, the temperature of the sintering treatment is 700-800° C.; the holding time of the sintering treatment is 9-12 hours.

[0052] For example, in different embodiments, the temperature of the sintering treatment may be 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, etc.; the holding time of the sintering treatment may be 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, etc.

[0053] In a specific embodiment of the present invention, the preparation of the Fe-MOF material includes: dispersing iron salt in a solution of an organic ligand, heating the solution at 140-180° C. for 6-12 hours, cooling the solution to room temperature, washing and drying the solution.

[0054] For example, in different embodiments, in the preparation of the Fe-MOF material, the temperature of the heating reaction can be exemplified by 140°C, 150°C, 160°C, 170°C, 180°C, etc., and the time of the heating reaction can be 6h, 7h, 8h, 9h, 10h, 11h, 12h, etc.

[0055] In actual operation, the reaction can be carried out in a high-pressure reactor.

[0056] In a specific embodiment of the present invention, the washing comprises: using anhydrous ethanol to centrifugally wash the material cooled to room temperature, preferably the washing times are ≥ 3 times.

[0057] In a specific embodiment of the present invention, the molar ratio of the iron salt to the organic ligand is 1:(0.5-2).

[0058] For example, in different embodiments, the molar ratio of the iron salt to the organic ligand can be exemplified as 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, etc.

[0059] In a specific embodiment of the present invention, the iron salt includes any one or more of ferric chloride, ferric nitrate and ferric sulfate.

[0060] In a specific embodiment of the present invention, the solution of the organic ligand is prepared by mixing the organic ligand and a solvent. Further, the solvent includes at least one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and the like.

[0061] In a specific embodiment of the present invention, in the Fe-MOF material, the organic ligands constituting the organic skeleton include at least one polycarboxylic acid organic ligand; the number of carboxylic acid groups in a single polycarboxylic acid organic ligand is ≥3.

[0062] By using an organic ligand having the above number of carboxylic acid groups, the obtained Fe-MOF material has a specific morphology, which can induce the preparation of a lithium iron phosphate positive electrode material with a fine particle size.

[0063] In a specific embodiment of the present invention, in the Fe-MOF material, the organic ligand constituting the organic framework includes trimesic acid.

[0064] In a specific embodiment of the present invention, the preparation of the Fe-MOF material further comprises: before the heating reaction, dispersing the iron salt in a solution of an organic ligand and ultrasonically treating the solution for 20 to 40 minutes.

[0065] In a specific embodiment of the present invention, the method further comprises: cooling the sintered material, and then grinding and sieving it. The mesh size of the sieving can be adjusted according to actual needs, such as 200-300 mesh sieve.

[0066] The present invention also provides a lithium iron phosphate positive electrode material prepared by using any one of the above-mentioned methods for preparing the lithium iron phosphate positive electrode material.

[0067] In a specific embodiment of the present invention, the average particle size of the lithium iron phosphate positive electrode material is 1.12-2.01 μm.

[0068] For example, in different embodiments, the average particle size of the lithium iron phosphate positive electrode material may be illustratively 1.12 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, etc.

[0069] In a specific embodiment of the present invention, the particle size concentration (D90-D10) / D50 of the lithium iron phosphate positive electrode material is 2.56-4.26.

[0070] For example, in different embodiments, the particle size concentration of the lithium iron phosphate positive electrode material is (D90-D10) / D50, and the results can be exemplified as 2.56, 2.6, 2.8, 3, 3.2, 3.4, 3.5, 3.6, 3.8, 4, 4.2, etc.

[0071] In a specific embodiment of the present invention, the powder resistivity of the lithium iron phosphate positive electrode material is 19.54 to 65.45 Ohm-cm under a pressure of 4 kN.

[0072] For example, in different embodiments, the resistivity of the lithium iron phosphate positive electrode material under a pressure of 4kN may be illustratively 19.54Ohm-cm, 20Ohm-cm, 25Ohm-cm, 30Ohm-cm, 35Ohm-cm, 40Ohm-cm, 45Ohm-cm, 50Ohm-cm, 55Ohm-cm, 60Ohm-cm, 65Ohm-cm, etc.

[0073] The present invention also provides a lithium-ion battery, comprising any one of the above-mentioned lithium iron phosphate positive electrode materials.

[0074] The lithium ion battery obtained by adopting the lithium iron phosphate positive electrode material of the present invention has excellent stability and rate performance.

[0075] Example 1

[0076] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:

[0077] (1) Preparation of Fe-MOF materials:

[0078] 2.1 g of trimesic acid (H3BTC) was weighed and fully dissolved in 200 mL of DMF to obtain a DMF solution of trimesic acid; then 2.71 g of FeCl3·6H2O was weighed and added to the DMF solution of trimesic acid, and after ultrasonic treatment for 20 min, it was moved into a polytetrafluoroethylene-lined high-pressure reactor, heated at 150°C for 12 h, cooled to room temperature, and washed three times by centrifugation with anhydrous ethanol. After drying and grinding, the precursor Fe-MOF material was obtained.

[0079] (2) Preparation of lithium iron phosphate positive electrode material:

[0080] Fe-MOF material and lithium dihydrogen phosphate are weighed at a molar ratio of 1:1 between Fe and P, 1 mol of Fe-MOF material (in terms of Fe) and 1 mol of lithium dihydrogen phosphate are mixed, and the mixture of Fe-MOF material and lithium dihydrogen phosphate is ball-milled at 2500 rpm for 8 hours using a high-speed ball mill; the ball-milled material is then placed in a high-temperature tubular furnace filled with argon, heat treated at 750°C for 12 hours, cooled to room temperature, ground to eliminate lumps, and sieved with a 200-mesh sieve to obtain a lithium iron phosphate positive electrode material.

[0081] Example 2

[0082] This example is based on the preparation method of Example 1, with the only difference being that in step (1), the amount of trimesic acid used is different.

[0083] In this embodiment, when preparing the Fe-MOF material, the amount of trimesic acid (H3BTC) used is 4.2 g.

[0084] Example 3

[0085] This example is prepared by referring to the method of Example 1, except that in step (1), the amount of FeCl3·6H2O used is different.

[0086] In this embodiment, when preparing the Fe-MOF material, the amount of FeCl3·6H2O used is 5.42 g.

[0087] Example 4

[0088] This example refers to the preparation method of Example 1, with the only difference being that in step (2), the molar ratio of the Fe-MOF material to lithium dihydrogen phosphate is different.

[0089] In this embodiment, when preparing the lithium iron phosphate positive electrode material, the molar ratio of the Fe-MOF material and lithium dihydrogen phosphate in terms of Fe and P respectively is 2:1.

[0090] Example 5

[0091] This example refers to the preparation method of Example 1, with the only difference being that in step (1), the amount of trimesic acid used is different; and in step (2), the molar ratio of the Fe-MOF material to lithium dihydrogen phosphate is different.

[0092] In this embodiment, when preparing the Fe-MOF material, the amount of trimesic acid (H3BTC) used is 4.2 g; when preparing the lithium iron phosphate positive electrode material, the molar ratio of the Fe-MOF material and lithium dihydrogen phosphate in terms of Fe and P respectively is 2:1.

[0093] Example 6

[0094] This example refers to the preparation method of Example 1, with the only difference being that in step (1), the amount of FeCl3·6H2O is different; and in step (2), the molar ratio of the Fe-MOF material to lithium dihydrogen phosphate is different.

[0095] In this embodiment, when preparing the Fe-MOF material, the amount of FeCl3·6H2O used is 5.42 g; when preparing the lithium iron phosphate positive electrode material, the molar ratio of the Fe-MOF material and lithium dihydrogen phosphate in terms of Fe and P respectively is 2:1.

[0096] Example 7

[0097] This example refers to the preparation method of Example 1, with the only difference being that in step (2), the temperature of the heat treatment is different.

[0098] In this embodiment, when preparing the lithium iron phosphate positive electrode material, the heat treatment temperature is 650°C.

[0099] Example 8

[0100] This example refers to the preparation method of Example 1, with the only difference being that in step (1), the organic ligand used to prepare the Fe-MOF material is different.

[0101] In this embodiment, when preparing the Fe-MOF material, the organic ligand trimesic acid (H3BTC) in Example 1 is replaced by an equal molar amount of the organic ligand terephthalic acid.

[0102] Comparative Example 1

[0103] Comparative Example 1 provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:

[0104] Iron oxide and lithium dihydrogen phosphate are weighed at a molar ratio of 1:1 based on Fe and P, 1 mol of iron oxide and 1 mol of lithium dihydrogen phosphate are mixed, and the mixture of iron oxide and lithium dihydrogen phosphate is ball-milled at 2500 rpm for 8 hours using a high-speed ball mill; the ball-milled material is then placed in a high-temperature tubular furnace filled with argon, heat-treated at 750°C for 8 hours, and then 0.1 mol of glucose is added and heat-treated at 750°C for 4 hours. After cooling to room temperature, the material is ground to eliminate lumps, and the material is sieved with a 200-mesh sieve to obtain a lithium iron phosphate positive electrode material.

[0105] Experimental Example 1

[0106] Figure 1 and Figure 2 They are XRD diagrams of lithium iron phosphate cathode materials prepared in Example 5 of the present invention and Comparative Example 1. As can be seen from the figure, the XRD diffraction peak position of LFP prepared by the method of the present invention corresponds to the XRD diffraction peak position of LFP prepared by the traditional method, indicating that the present method can be used to effectively synthesize LFP cathode materials.

[0107] The lithium iron phosphate positive electrode material prepared in Example 5 is taken as an example for description. The lithium iron phosphate positive electrode material prepared in Example 5 is in the form of zero-dimensional spherical particles.

[0108] The average particle size, particle concentration and powder conductivity of the lithium iron phosphate positive electrode materials prepared in each embodiment and comparative example were characterized by a laser particle size analyzer and a powder resistivity meter. The results are shown in Table 1.

[0109] Table 1 Test results of different lithium iron phosphate cathode materials

[0110]

[0111] As can be seen from Table 1, the present invention uses Fe-MOF as an iron source, which can achieve multiple effects such as refining material grains, ensuring particle uniformity, and improving the conductivity of the material.

[0112] Experimental Example 2

[0113] The materials prepared in Example 5 and Comparative Example 1 were respectively used to assemble button batteries in a glove box using lithium sheets as counter electrodes. Specifically, a 12 μm thick carbon-coated aluminum foil was used as the current collector, and a slurry was prepared according to the mass ratio of positive electrode material: SP: PVDF = 96:2:2. The coating surface density of the electrode sheet was 15 mg / cm 2 , lithium sheet was used as counter electrode. Then the electrochemical performance was tested using a blue electric test system and an electrochemical workstation, and the results are shown in Table 2.

[0114] Table 2 Power-off test results

[0115]

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The steps include: The iron source, phosphorus source and lithium source are mixed and ground, and then sintered under a protective atmosphere; The iron source includes Fe-MOF material; The sintering temperature is 740-760°C; the sintering holding time is 10-12h; The lithium iron phosphate positive electrode material is in the form of zero-dimensional spherical particles; the particle size concentration (D90-D10) / D50 of the lithium iron phosphate positive electrode material is 2.56-4; In the Fe-MOF material, the organic ligand constituting the organic framework is trimesic acid; The preparation of the Fe-MOF material comprises: dispersing iron salt in a solution of an organic ligand, heating at 140-180° C. for a reaction of 6-12 hours, cooling, washing and drying; The molar ratio of the iron salt to the organic ligand is 1:(0.5-2).

2. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The molar ratio of the iron source, the phosphorus source and the lithium source used, calculated as Fe, P and Li, is (1-2): (0.8-1.2):

1.

3. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The phosphorus source includes any one or more of diammonium phosphate, diammonium hydrogen phosphate and lithium dihydrogen phosphate; And / or, the lithium source includes any one or more of lithium carbonate, lithium hydroxide, lithium oxalate and lithium dihydrogen phosphate.

4. The method for preparing a lithium iron phosphate positive electrode material according to claim 1, characterized in that: The grinding is ball milling.

5. The method for preparing the lithium iron phosphate positive electrode material according to claim 4, characterized in that: The ball milling time is 4 to 12 hours.

6. The method for preparing the lithium iron phosphate positive electrode material according to claim 4, characterized in that: The rotation speed of the ball mill is 1000-4000 rpm.

7. A lithium iron phosphate positive electrode material prepared by the method for preparing a lithium iron phosphate positive electrode material according to any one of claims 1 to 6.

8. The lithium iron phosphate positive electrode material according to claim 7, characterized in that: Having at least one of the following characteristics: (a) The average particle size of the lithium iron phosphate positive electrode material is 1.12-2.01 μm; (b) The powder resistivity of the lithium iron phosphate positive electrode material is 19.54~65.45Ohm-cm under a pressure of 4kN.

9. A lithium-ion battery, characterized in that Comprising the lithium iron phosphate positive electrode material as described in claim 7 or 8.

Citation Information

Cited By

  • A lithium iron phosphate positive electrode material and its preparation method and application

    CN119218969B