A high entropy alloy material and coating for thermal control coating and preparation method thereof
High-entropy alloy materials composed of nickel, cobalt, chromium, manganese and non-metallic elements, combined with atmospheric plasma spraying technology, solve the shortcomings of existing thermal control coatings in heating efficiency and stability, and achieve high resistivity and high The combined strength of the coating significantly improves the overall performance of the thermal control coating.
Patent Information
- Application Number
- CN202211288455.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Existing electric heating technology has problems in the field of thermal control such as low heating efficiency, complex assembly, uneven heating, and the brittleness of ceramic coatings that easily peel off. Research on the electrothermal properties of high-entropy alloys is relatively limited, especially the comprehensive performance of thermal spray coatings. reach a satisfactory level.
High-entropy alloy material composed of 15-20% nickel, 13-20% cobalt, 13-18% chromium, 13-20% manganese and 0.05-2% non-metallic elements (boron and/or silicon) is sprayed by atmospheric plasma The process prepares high-resistance coatings, optimizing the composition and process parameters to improve the resistivity, bonding strength and hardness of the coating, and achieve a single-phase structure and high heating efficiency.
The resistivity, bonding strength and hardness of the coating are significantly improved. The resistivity can exceed 350μΩ·cm and the bonding strength exceeds 35MPa. The heating efficiency and reliability of the coating are greatly improved. The process is simple and does not require complicated casting, forging and drawing processes. .
Smart Images

Figure CN116024478B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of surface coatings, and in particular to a high entropy alloy material and coating for thermal control coatings and a preparation method thereof. Background Art
[0002] Traditional alloys are generally based on a single element, while high entropy alloys break through this traditional design concept and use multiple elements as the main element, with the atomic percentage of each main element being 5% to 35%. Compared with traditional alloys, high entropy alloys have the potential to obtain excellent properties such as good strength, conductivity, hardness, wear resistance, corrosion resistance and thermal stability due to their high entropy effect, hysteresis diffusion effect, lattice distortion effect and cocktail effect. At present, the preparation and research of high entropy alloys are mainly focused on bulk alloys used as structural materials. There are relatively few studies involving coatings, and the research is mainly focused on the wear and corrosion resistance of coatings. The preparation methods used are mostly laser / plasma cladding and other processes.
[0003] Thermal control technology is mainly divided into passive thermal control technology and active thermal control technology. Common active thermal control technologies include electric heating technology, single-phase fluid circuit technology, two-phase fluid circuit technology and ventilation cooling technology. The heaters of electric heating technology mainly involve organic material heating plates or ceramic heating layers or resistance wire heating. However, resistance wire heating technology generally has problems such as low heating efficiency, complex assembly, and uneven heating. Ceramic coatings are prone to peeling due to the brittle properties of ceramic materials and low bonding strength. Organic material patches are prone to aging and other phenomena under long-term use conditions, and then fail.
[0004] Metals and alloy materials are considered to be good conductors, so researchers pay relatively limited attention to the electrothermal properties of alloys, especially for thermal spray coatings. The metal heating coating technology proposed by the inventor's research team in recent years can effectively overcome the shortcomings of the above-mentioned electric heating technologies. A high-entropy alloy powder, high-resistance coating, preparation method and application thereof (ZL 202010553534.2) previously applied for can reach a room temperature resistivity of 300-330μΩ·cm, but for application environments with high energy utilization requirements, the heating efficiency and comprehensive effect of the coating still need to be further improved. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a high entropy alloy material and coating for thermal control coating and a preparation method thereof.
[0006] In a first aspect, the present invention provides a high entropy alloy material for a thermal control coating, wherein the high entropy alloy material comprises the following components in percentage by mass: 15-20% nickel, 13-20% cobalt, 13-18% chromium, 13-20% manganese, 0.05-2% non-metallic elements, and iron as the balance; wherein the non-metallic elements are boron and / or silicon.
[0007] The high entropy alloy material provided by the present invention is combined with the coating process of the present invention to achieve the optimized design of interstitial solid solution enhanced high entropy alloy coating resistivity. Through the optimized design of the high entropy alloy material, the specific amounts and combinations of non-metallic elements (Si, B), nickel, cobalt, chromium, manganese and iron are used. Under the coating preparation process conditions of the present invention, the coating performance can achieve higher resistivity while the oxygen content is further reduced, and the coating hardness and bonding strength are higher, so that the comprehensive performance of the metal thermal control coating is significantly improved.
[0008] Preferably, the high entropy alloy material for thermal control coating has the following composition in percentage by mass: 15-20% nickel, 13-17% cobalt, 14-18% chromium, 13-18% manganese, 0.2-1.6% non-metallic elements, iron as the balance, and unavoidable impurities; the non-metallic elements are boron and / or silicon. Preferably, the high entropy alloy material is used for the preparation of high entropy alloy coatings with high resistivity and high bonding strength.
[0009] Further preferably, the composition of the high entropy alloy material for thermal control coating is as follows by mass percentage: nickel 15-18%, cobalt 16-17%, chromium 14-17%, manganese 13-14%, boron 0.08-0.4%, silicon 0.2-0.8%, iron as the balance, and inevitable impurities; the high entropy alloy material is preferably used for the preparation of metal thermal control coatings with high resistivity and high bonding strength, preferably, the resistivity is greater than 350μΩ·cm, such as 380μΩ·cm, 400μΩ·cm, 405μΩ·cm, and the bonding strength is 35-38MPa, such as 36.5MPa, 37.1MPa. Further preferably, the high entropy alloy material is an alloy powder with a particle size of 38-75μm. The high entropy alloy material optimized by the present invention is used as the raw material of the metal thermal control coating, which has better comprehensive performance than the existing high entropy alloy powder for metal thermal control coating.
[0010] In a second aspect, the present invention provides a metal thermal control coating, wherein the high resistance coating is prepared from the high entropy alloy material by a thermal spraying method.
[0011] In the present invention, by adopting the specific composition and content of the preferred high entropy alloy material in combination with a specific preparation process, the high-resistance coating used in the field of electric heating can obtain a better single-phase structure while further improving the coating resistance, so that the resistivity performance is better and the heating efficiency is higher, while achieving better performance in terms of porosity, oxygen content, bonding strength, etc.
[0012] Preferably, the metal thermal control coating is prepared by the high entropy alloy material for thermal control coating through an atmospheric plasma spraying process, and the composition of the metal thermal control coating / high entropy alloy material in terms of mass percentage is as follows: nickel 15-16%, cobalt 16-17%, chromium 14-15%, manganese 13-14%, boron 0.1-0.2%, silicon 0.2-0.3%, iron as the balance, and unavoidable impurities.
[0013] Further preferably, the composition by mass percentage is as follows: nickel 16%, cobalt 17%, chromium 14%, manganese 13%, boron 0.1%, silicon 0.2%, iron as the balance, and inevitable impurities. Preferably, the spraying process parameters in the preparation process of the atmospheric plasma spraying process are: current: 600-650A, argon flow rate: 41-45L / min, hydrogen flow rate: 4-8L / min, powder feeding rate: 50-60g / min, spraying distance: 90-110mm. The present invention can achieve unexpected comprehensive effect improvement based on the synergistic cooperation of each component in a specific amount combined with specific spraying process parameters.
[0014] In the third aspect, the present invention provides a method for preparing the metal thermal control coating, wherein the high entropy alloy material with a particle size range of 38 to 75 μm is subjected to an atmospheric plasma spraying process to prepare the metal thermal control coating, and the spraying process parameters are: current: 600 to 650 A, argon flow rate: 41 to 45 L / min, hydrogen flow rate: 4 to 8 L / min, powder feeding rate: 50 to 60 g / min, and spraying distance: 90 to 110 mm.
[0015] Preferably, the spraying process parameters are: current: 600-620A, argon flow rate: 41-45L / min, hydrogen flow rate: 6-8L / min, powder feeding rate: 55-60g / min, spraying distance: 100-110mm.
[0016] Further preferably, the spraying process parameters are: current: 605-615A, argon flow rate: 44-45L / min, hydrogen flow rate: 6-7L / min, powder feeding rate: 57-59g / min, spraying distance: 105-110mm.
[0017] In the present invention, through the joint optimization of the metal coating material and process parameters of the metal thermal control coating, especially the combination of the design of specific component composition and content and the preferred process parameters, the metal thermal control coating obtained by the present invention can have the best comprehensive performance in terms of resistivity, oxygen content, bonding strength, hardness and porosity, and has better coating heating efficiency, comprehensive effect and reliability.
[0018] In a third aspect, the present invention provides the application of the high entropy alloy material for thermal control coating, the metal thermal control coating, or the metal thermal control coating prepared by the preparation method of the metal thermal control coating in active thermal control metal coating.
[0019] In the present invention, the phase structure of the metal thermal control coating (high resistance alloy coating) is a single-phase solid solution, but has high resistance. The improvement of the coating resistance performance is due to the reasonable combination of the design of the composition and the preparation method. The coating material in the present invention is a multi-principal alloy containing nickel, iron, cobalt, chromium and manganese and non-metallic elements boron and silicon. The design of several transition metals is based on the consideration that their atomic radii are relatively close and can achieve better mutual dissolution, in order to obtain a single-phase solid solution structure, so that the material can have better process adaptability, that is, it has better plastic deformation ability to keep the coating in good compactness; at the same time, the larger lattice distortion of the multi-principal alloy can also improve the overall resistivity; chromium is beneficial to improve the overall corrosion resistance of the coating; manganese is necessary to increase the lattice distortion of the alloy system, reduce the stacking fault energy, and reduce the ferromagnetic properties of the coating; non-metallic elements boron and / or silicon can refine the grains, increase the grain boundary density, and improve the overall resistivity of the coating on the one hand, and non-metallic elements combined with the spraying process characteristics can play a deoxidation role of flying particles and reduce the oxide content in the coating. The overall improvement of coating resistance is mainly achieved through the rational configuration of the alloy's own components and the combined effect of the preparation method. It is not determined by any single element, but it is also indispensable. Of course, it cannot be achieved through just a limited number of tests.
[0020] The beneficial effects of the present invention are at least: 1) the alloy coating maintains a single-phase FCC stable phase structure; 2) the oxygen content in the coating is as low as below 2wt.%; 3) the resistivity of the coating is significantly improved, which can exceed 350μΩ·cm, which is higher than the traditional nickel-chromium alloy resistance wire material (about 100-115μΩ·cm); 4) the bonding strength of the alloy coating exceeds 35MPa; 5) the hardness is significantly improved, which can reach above 350HV; 6) the preparation method is simple, and does not require casting, forging, drawing and other processing involved in the resistance wire preparation process; 7) the coating heating efficiency and reliability are higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is the X-ray diffraction (XRD) spectrum of the coating provided in Example 2 of the present invention.
[0023] Figure 2 This is a metallographic morphology image of the coating provided in Example 2 of the present invention.
[0024] Figure 3 This is a metallographic morphology image of the coating provided for Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer is not specified for the instruments used, they are all conventional products that can be purchased through regular channels. The methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used.
[0027] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0028] In the following example:
[0029] (1) Raw material selection: The purity of nickel, iron, cobalt, chromium, manganese, boron and silicon is 99.6wt.% respectively.
[0030] (2) preparing powder of alloy material by nitrogen atomization method, collecting powder with particle size ranging from 38 to 75 μm for atmospheric plasma spraying;
[0031] (3) The substrate is aluminum alloy, and its surface is pretreated to remove the surface oxide film and dirt, and then sandblasted;
[0032] (4) The powder in step 2 is subjected to an atmospheric plasma spraying process to prepare an alloy coating having a coating thickness of 350 to 500 μm.
[0033] (5) The prepared alloy powder material and coating were subjected to microstructure characterization, resistivity, hardness and bonding strength performance tests under the same conditions: the phase structure was characterized by an X-ray diffractometer (D8 Advance) from Bruker, and the surface area of the test sample was 10×10mm 2 ; Microstructure observation was performed using an OLMPUS PMG3 optical microscope; resistivity test was performed using a four-point probe method, using the PPMS-9 test system from the American Quantum Design Company, and the sample size was 5×2×0.5mm 3 ; The hardness of the coating section was tested using an MH-3 microhardness tester with a load of 100g and a loading time of 15s. The test was performed 15 times to take the average value. The coating bonding strength test was based on the test standard: ASTMC633-01. Both the specimen and the loading rod were made of 4032 aluminum alloy. The bonding material was high-temperature structural adhesive E-7 adhesive with a tensile strength of 70MPa. The curing condition was maintained at 110°C for 3h and the test was performed at room temperature. The experimental equipment was Changchun Qianbang QBD-100.
[0034] Example 1
[0035] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 15%, cobalt: 17%, chromium: 18%, manganese: 18%, boron: 0.08%, silicon: 0.5%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 600A, argon flow rate: 41L / min, hydrogen flow rate: 8L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0036] Example 2
[0037] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 16%, cobalt: 17%, chromium: 14%, manganese: 13%, boron: 0.1%, silicon: 0.2%, iron: balance, and inevitable impurities. Spraying process parameters are: current: 610A, argon flow: 45L / min, hydrogen flow: 6L / min, powder feeding rate: 58g / min, spraying distance: 110mm. The X-ray diffraction (XRD) spectrum of this embodiment is shown in Figure 1 As shown, the metallographic morphology is as follows Figure 2 shown.
[0038] Example 3
[0039] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 15%, cobalt: 17%, chromium: 18%, manganese: 18%, silicon: 0.2%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 610A, argon flow rate: 45L / min, hydrogen flow rate: 6L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0040] Example 4
[0041] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 16%, cobalt: 17%, chromium: 14%, manganese: 13%, boron: 0.1%, silicon: 0.2%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 610A, argon flow rate: 41L / min, hydrogen flow rate: 8L / min, powder feeding rate: 58g / min, spraying distance: 90mm.
[0042] Example 5
[0043] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 18%, cobalt: 13%, chromium: 18%, manganese: 13%, boron: 0.4%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 620A, argon flow rate: 41L / min, hydrogen flow rate: 8L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0044] Example 6
[0045] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 16%, cobalt: 17%, chromium: 18%, manganese: 18%, silicon: 0.8%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 600A, argon flow rate: 45L / min, hydrogen flow rate: 8L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0046] Example 7
[0047] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 17%, cobalt: 17%, chromium: 17%, manganese: 18%, boron: 0.5%, silicon: 0.8%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 600A, argon flow rate: 41L / min, hydrogen flow rate: 6L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0048] Example 8
[0049] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 20%, cobalt: 17%, chromium: 18%, manganese: 13%, boron: 0.4%, silicon: 1.2%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 600A, argon flow rate: 45L / min, hydrogen flow rate: 6L / min, powder feeding rate: 58g / min, spraying distance: 90mm.
[0050] Example 9
[0051] The chemical composition and mass percentage of the alloy material in this embodiment are: nickel: 17%, cobalt: 17%, chromium: 18%, manganese: 18%, boron: 0.4%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 650A, argon flow rate: 45L / min, hydrogen flow rate: 4L / min, powder feeding rate: 58g / min, spraying distance: 110mm.
[0052] Comparative Example 1
[0053] The chemical composition and mass percentage of the alloy material in this comparative example are: nickel: 18%, cobalt: 18%, chromium: 20%, manganese: 17%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 500A, argon flow rate: 35L / min, hydrogen flow rate: 12L / min, powder feeding rate: 60g / min, spraying distance: 120mm.
[0054] Comparative Example 2
[0055] The chemical composition and mass percentage of the alloy material in this comparative example are: nickel: 21%, cobalt: 12%, chromium: 12%, manganese: 22%, boron: 0.02%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 610A, argon flow rate: 45L / min, hydrogen flow rate: 6L / min, powder feeding rate: 58g / min, spraying distance: 110mm. Figure 3 This is the metallographic morphology of Comparative Example 2.
[0056] Comparative Example 3
[0057] The chemical composition and mass percentage of the alloy material in this comparative example are: nickel: 18%, cobalt: 18%, chromium: 20%, manganese: 17%, boron: 0.4%, silicon: 2.0%, iron: balance, and inevitable impurities. The spraying process parameters are: current: 500A, argon flow rate: 35L / min, hydrogen flow rate: 6L / min, powder feeding rate: 60g / min, spraying distance: 120mm.
[0058] The test results of the coating phase structure, porosity, oxygen content, hardness, bonding strength and resistivity of Examples 1-9 and Comparative Examples 1-3 are shown in Table 1.
[0059] Table 1 Coating performance test results of the embodiments and comparative examples
[0060]
[0061] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A metal thermal control coating, characterized in that: The metal thermal control coating is prepared from a high entropy alloy material by an atmospheric plasma spraying process, wherein the composition of the high entropy alloy material by mass percentage is as follows: 15-16% nickel, 16-17% cobalt, 14-15% chromium, 13-14% manganese, 0.1-0.2% boron, 0.2-0.3% silicon, iron as the balance, and unavoidable impurities; The spraying process parameters are: current: 600~620A, argon flow rate: 41~45L / min, hydrogen flow rate: 6~8L / min, powder feeding rate: 55~60g / min, spraying distance: 100~110mm; the metal thermal control coating is a high-resistivity metal-based active thermal control coating with a resistivity greater than 400μΩ·cm.
2. The metal thermal control coating according to claim 1, characterized in that: The high entropy alloy material is an alloy powder with a particle size of 38 to 75 μm.
3. The metal thermal control coating according to claim 1, characterized in that: The composition by mass percentage is as follows: nickel 16%, cobalt 17%, chromium 14%, manganese 13%, boron 0.1%, silicon 0.2%, iron as the balance, and inevitable impurities.
4. The method for preparing the metal thermal control coating according to any one of claims 1 to 3, characterized in that: The high entropy alloy material with a particle size range of 38~75μm is used to prepare a metal thermal control coating by an atmospheric plasma spraying process, and the spraying process parameters are: current: 600~620A, argon flow rate: 41~45L / min, hydrogen flow rate: 6~8L / min, powder feeding rate: 55~60g / min, and spraying distance: 100~110mm.
5. Use of the metal thermal control coating according to any one of claims 1 to 3 or the metal thermal control coating prepared by the preparation method of the metal thermal control coating according to claim 4 in active thermal control metal coatings.