A high-flux, anti-pollution reverse osmosis membrane, preparation method and application thereof

By using indene compounds containing amino and carboxyl structures in the reverse osmosis membrane for interfacial polymerization reaction with 2-naphthoyl chloride, combined with sodium hypochlorite water treatment, the problem of taking into account both the flux and anti-pollution performance of the reverse osmosis membrane is solved, and high Improved flux, high desalination rate and anti-pollution performance are suitable for water treatment.

CN116036878BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310000444.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-12-03
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

Existing reverse osmosis membranes are difficult to balance between improving flux and anti-pollution properties, and the membrane surface is susceptible to contaminants and chemical degradation.

Method used

By adding indene compounds containing amino and carboxyl structures and 2-naphthoyl chloride to the aqueous and organic phase solutions, it participates in the interfacial polymerization reaction to form a modified polyamide separation layer, combined with sodium hypochlorite water post-treatment and moisturizing drying, it is prepared A large-flux, pollution-resistant reverse osmosis membrane is produced.

Benefits of technology

The high throughput, high desalination rate and excellent anti-pollution properties of the reverse osmosis membrane are achieved, which enhances the comprehensive performance of the membrane and simplifies the preparation process, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004034246900000081
    Figure BDA0004034246900000081
  • Figure BDA0004034246900000101
    Figure BDA0004034246900000101
  • Figure BDA0004034246900000102
    Figure BDA0004034246900000102
Patent Text Reader

Abstract

The invention discloses a high-flux anti-pollution reverse osmosis membrane and a preparation method thereof. The method comprises the following steps: 1) adding an indene compound containing an amino group and a carboxyl group and 2-naphthoyl chloride to an aqueous solution containing m-phenylenediamine and an organic phase containing trimesoyl chloride, respectively, and stirring evenly to obtain an aqueous phase solution and an oil phase solution; 2) contacting a polysulfone-based membrane with an aqueous phase and an oil phase solution, respectively, and generating an interfacial polymerization reaction to generate a modified polyamide separation layer to obtain a basic reverse osmosis membrane; 3) immersing the basic reverse osmosis membrane in a sodium hypochlorite water tank for post-treatment, moisturizing treatment and drying to obtain a high-flux anti-pollution reverse osmosis membrane. The present invention introduces an indene compound containing an amino group and a carboxyl group and 2-naphthoyl chloride, and cross-polymerizes with an amine monomer in the aqueous phase and an acyl chloride monomer in the oil phase to obtain a modified polyamide separation layer with an interlocking structure and a surface modified with a special functional group, which gives the reverse osmosis membrane excellent anti-pollution performance, and at the same time has a high water flux and desalination rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of separation membranes, and in particular to a large-flux, pollution-resistant reverse osmosis membrane, a preparation method and application thereof. Background Art

[0002] With the rapid development of the world economy, the demand for fresh water resources is increasing. Separation membrane technology has received widespread attention and is expected to alleviate the water crisis.

[0003] The core of separation membrane technology is osmotic membrane, and reverse osmosis membrane is the most successful case of commercialization of osmotic membrane. Although the technology application has been developed and accumulated for many years, there are still some problems with the membrane itself. For example, on the one hand, it is difficult to obtain an ideal water production flux while ensuring high selectivity of salt ions; on the other hand, the membrane surface is easily blocked and chemically degraded by pollutants. Therefore, it is the direction of many researchers' efforts to prepare a modified polyamide separation layer through interfacial polycondensation reaction to obtain a reverse osmosis membrane with high flux, high salt removal rate and excellent anti-pollution performance.

[0004] In order to improve the flux and salt rejection of reverse osmosis membrane, currently disclosed patents mainly add different types of additives to aqueous phase solution or organic phase solution, and improve performance by optimizing interfacial polycondensation to improve polyamide layer structure. For example, in patents such as US5254261, US6171497, US687827, CN1328483A, flux improvement is achieved by adding additives to polyamine aqueous phase solution or organic phase solution. In order to improve the anti-pollution ability of reverse osmosis membrane, commonly used modification methods are physicochemical methods such as membrane surface coating (such as CN1213985A, method disclosed in CN101450290A), surface chemical modification (method disclosed in CN104785131), surface grafting (method disclosed in CN104815567A), so as to improve the anti-pollution performance of reverse osmosis composite membrane by changing the surface hydrophilicity, surface roughness and surface charge of reverse osmosis membrane.

[0005] Although the prior art has formed some technical solutions for improving the water flux and / or anti-fouling performance of reverse osmosis membranes, these technical solutions still need to be further improved in terms of improving the anti-fouling performance of reverse osmosis membranes while maintaining high flux.

[0006] Therefore, there is still an urgent need to develop a reverse osmosis membrane with high flux, high desalination and excellent anti-fouling performance. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a high-flux, anti-pollution reverse osmosis membrane, so as to prepare a reverse osmosis membrane with high flux, high desalination and excellent anti-pollution performance.

[0008] Another object of the present invention is to provide such a high-flux, anti-fouling reverse osmosis membrane.

[0009] Another object of the present invention is to provide the application of such high-flux, anti-fouling reverse osmosis membrane.

[0010] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0011] A method for preparing a high-flux, anti-pollution reverse osmosis membrane comprises the following steps:

[0012] 1) adding an indene compound containing an amino group and a carboxyl group structure to an aqueous solution containing m-phenylenediamine, and stirring the mixture to obtain an aqueous phase solution; adding 2-naphthoyl chloride to an organic phase containing trimesoyl chloride, and stirring the mixture to obtain an oil phase solution;

[0013] 2) contacting the polysulfone-based membrane with the aqueous solution and the oily solution respectively, causing interfacial polymerization to form a modified polyamide separation layer, thereby obtaining a basic reverse osmosis membrane;

[0014] 3) The basic reverse osmosis membrane is immersed in a sodium hypochlorite water tank for post-treatment, moisturizing treatment and drying to obtain the high-flux, anti-pollution reverse osmosis membrane.

[0015] In a specific embodiment, the aqueous solution in step 1) contains 0.1-2.0 wt% of indene compounds containing amino and carboxyl structures. Preferably, the mass concentration of indene compounds containing amino and carboxyl structures in the aqueous solution is 0.5%-1.0%; more preferably, the indene compounds containing amino and carboxyl structures are selected from one or both of 1-aminoindene-1-carboxylic acid and 2-aminoindene-2-carboxylic acid.

[0016] In a specific embodiment, in the aqueous solution of step 1), the mass percentage of m-phenylenediamine is 1.5-5.0 wt %.

[0017] In a specific embodiment, the mass concentration of 2-naphthoyl chloride in the oil phase solution of step 1) is 0.02-0.2 wt%, preferably 0.05-0.1% wt%.

[0018] In a specific embodiment, the mass concentration of trimesoyl chloride in the oil phase solution of step 1) is 0.1-0.3%wt%.

[0019] In a specific embodiment, the contact time between the polysulfone-based membrane and the aqueous solution in step 2) is 10 s-120 s, preferably 30-60 s.

[0020] In a specific embodiment, the interfacial polymerization reaction time in step 2) is 2-60 s, preferably 10-30 s.

[0021] In a specific embodiment, the concentration of the sodium hypochlorite solution in the post-treatment water tank in step 3) is 50-500 ppm; preferably, the pH of the sodium hypochlorite solution in the water tank is 3-10.

[0022] In a specific embodiment, in step 3), glycerol or citric acid is used as a moisturizing agent in the moisturizing treatment, and the mass concentration of the moisturizing agent is preferably 1%-20wt%; preferably, the drying temperature is 60-90°C, and the drying time is 30-180s.

[0023] On the other hand, a high-flux, anti-fouling reverse osmosis membrane prepared by the aforementioned preparation method.

[0024] On the other hand, a high-flux, anti-fouling reverse osmosis membrane prepared by the aforementioned preparation method or the aforementioned is used in separation membranes or water treatment.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The preparation method of the present invention can directly participate in the interfacial polymerization process by adding indene compounds and 2-naphthoyl chloride containing amino and carboxyl structures, forming an interlocking structure with the bulk polymer, reorganizing the molecular network structure, making the membrane denser, and greatly improving the retention capacity of the membrane. In particular, the carboxylic acid groups contained therein increase the hydrophilicity of the membrane surface, which is conducive to the formation of a water layer on the membrane surface and the faster speed of water transporting through the channels in the membrane. The formation of the surface water layer makes it more difficult for pollutants to deposit on the membrane surface, thus playing an anti-pollution role. The faster speed of water transporting through the channels in the membrane results in a greater flux of the membrane.

[0027] (2) The preparation method of the present invention can not only make the prepared reverse osmosis membrane have a larger flux and a higher desalination rate, but also effectively improve the anti-pollution performance of the reverse osmosis membrane, thereby greatly enhancing the comprehensive performance of the reverse osmosis membrane.

[0028] (3) The present invention provides a method for preparing a large-flux anti-pollution reverse osmosis membrane, which is simple to operate and easy to industrialize.

[0029] (4) The reverse osmosis membrane provided by the present invention has the characteristics of anti-pollution, high flux and high desalination rate, which can further improve the treatment efficiency in water treatment fields such as household water purification and industrial water supply, and reduce operation and maintenance costs. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0031] A method for preparing a high-flux, anti-pollution reverse osmosis membrane comprises the following steps:

[0032] 1) adding an indene compound having an amino group and a carboxyl group and 2-naphthoyl chloride to an aqueous solution containing m-phenylenediamine and an organic phase containing trimesoyl chloride, respectively, and stirring to obtain an aqueous phase solution and an oil phase solution;

[0033] 2) contacting the polysulfone-based membrane with the aqueous phase and the oil phase solution respectively, causing interfacial polymerization to form a modified polyamide separation layer, thereby obtaining a basic large-flux anti-fouling reverse osmosis membrane;

[0034] 3) The basic large-flux anti-pollution reverse osmosis membrane is immersed in a sodium hypochlorite water tank for post-treatment, moisturizing treatment and drying to obtain a large-flux, anti-pollution reverse osmosis membrane.

[0035] The aqueous solution in step 1) contains an indene compound containing an amino group and a carboxyl group in a concentration of 0.1 to 2.0 wt%. For example, the mass concentration of the indene compound includes but is not limited to 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, preferably 0.5% to 1.0%.

[0036] The indene compound containing amino and carboxyl structures is, for example, one or more of 1-aminoindene-1-carboxylic acid and 2-aminoindene-2-carboxylic acid.

[0037] In the aqueous solution, the mass percentage of metaphenylenediamine is 1.5-5.0wt%, for example, including but not limited to 1.5wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.5wt%, 2.6wt%, 2.8wt%, 3.0wt%, 3.3wt%, 3.5wt%, 3.7wt%, 3.8wt%, 4.0wt%, 4.4wt%, 4.5wt%, 4.6wt%, 4.7wt%, 4.8wt%, 4.9wt%, and 5.0wt%.

[0038] In the aqueous phase solution, in addition to the aforementioned indene compounds containing amino and carboxyl structures and m-phenylenediamine, the balance is water.

[0039] In the oil phase solution of step 1), the mass concentration of 2-naphthoyl chloride is 0.02-0.2wt%, for example, but not limited to 0.02wt%, 0.04wt%, 0.06wt%, 0.08wt%, 0.1wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt%, 0.2wt%, preferably 0.05-0.1%wt%.

[0040] In the oil phase solution, the mass concentration of trimesoyl chloride is 0.1-0.3%wt, for example, including but not limited to 0.1wt%, 0.12wt%, 0.13wt%, 0.14wt%, 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt%, 0.19wt%, 0.2wt%, 0.21wt%, 0.22wt%, 0.23wt%, 0.24wt%, 0.25wt%, 0.26wt%, 0.27wt%, 0.28wt%, 0.29wt%, 0.3wt%, preferably 0.1-0.2wt%.

[0041] In the oil phase solution, in addition to the aforementioned 2-naphthoyl chloride and trimesoyl chloride, the balance is a solvent, which is usually an aliphatic alkane, such as any one of n-decane, n-hexane, and ISOPAR-G isoalkane, preferably ISOPAR-G isoalkane.

[0042] In step 2) of the present invention, the polysulfone-based membrane is a polysulfone support membrane formed on a non-woven fabric. The finished product can be directly purchased through commercial channels, or a polysulfone casting solution can be obtained by dissolving a polysulfone resin and ethylene glycol monomethyl ether in dimethylformamide; the polysulfone casting solution after filtration and degassing is then applied to a polyester non-woven fabric, and then put into water to form a membrane through phase transformation, and the polysulfone support membrane is obtained after washing. This is a known technology to those skilled in the art.

[0043] In this step, the polysulfone-based membrane is contacted with the aqueous phase and the oil phase solution respectively to generate an interfacial polymerization reaction to form a modified polyamide separation layer, that is, the aqueous phase is first contacted, and then the oil phase is contacted and the interfacial polymerization reaction occurs in the oil phase. Wherein, the contact (immersion) time of the polysulfone-based membrane in the aqueous phase solution is 10s-120s, for example, including but not limited to 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s, 65s, 70s, 75s, 80s, 85s, 90s, 95s, 100s, 105s, 110s, 115s, 120s, preferably 30-60s.

[0044] The interfacial polymerization reaction time in the oil phase is 2-60s, for example including but not limited to 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s, preferably 10-30s.

[0045] In step 3) of the present invention, the obtained basic reverse osmosis membrane is subjected to post-treatment, and the post-treatment step can refer to the prior art, and the present invention has no particular limitation. For example, it is immersed in a water tank containing a sodium hypochlorite solution for treatment, and the concentration of the sodium hypochlorite solution in the water tank is 10-1000ppm, for example, including but not limited to 10ppm, 50ppm, 100ppm, 150ppm, 200ppm, 250ppm, 300ppm, 350ppm, 400ppm, 450ppm, 500ppm, 550ppm, 600ppm, 650ppm, 700ppm, 750ppm, 800ppm, 850ppm, 900ppm, 950ppm, 1000ppm, preferably 50-500ppm; the pH of the sodium hypochlorite solution in the water tank is 3-10, for example, including but not limited to 3, 4, 5, 6, 7, 8, 9, 10, preferably pH 5-8.

[0046] The purpose of the sodium hypochlorite solution treatment is to oxidize the polyamide separation layer to improve the membrane performance. After the sodium hypochlorite solution post-treatment, a moisturizing treatment is further performed, and a moisturizing unit is used to perform a moisturizing treatment with a moisturizing agent. For example, glycerol or citric acid is used as a moisturizer. The mass concentration of the moisturizer is 1%-20wt%, for example, including but not limited to 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%. After the moisturizing treatment, the product is dried again. The drying temperature is, for example, 60-90°C, for example, 60°C, 70°C, 80°C, 90°C, etc.; the drying time is, for example, 30-180s, for example, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, 160s, 170s, 180s, etc.

[0047] The high-flux, anti-pollution reverse osmosis membrane prepared by the method of the present invention can be applied to water treatment, especially in water treatment components or devices. The water treatment component or device can be any component or device installed with the anti-pollution and oxidation-resistant polyamide reverse osmosis membrane of the present invention that can be applied to the water treatment process. The "applied in water treatment components or devices" includes the application to the component or device product installed with the anti-pollution polyamide reverse osmosis membrane of the present invention, and also includes the application to the preparation of such component or device products. The components can be, for example, spiral membrane components and disc-tube flat membrane components. The devices can be, for example, household / commercial reverse osmosis water purifiers, industrial boiler feed water reverse osmosis pure water devices, industrial water reuse reverse osmosis devices, and seawater desalination devices. The water treatment methods can be, for example: methods for drinking water production, wastewater reuse, seawater desalination, beverage concentration, etc.

[0048] Unless otherwise specified, the raw materials used in the following examples or comparative examples are all commercially available industrial-grade conventional raw materials. The main raw material information is shown in Table 1 below.

[0049] Table 1 Main raw materials

[0050] Raw material name Parameters Manufacturer Metaphenylenediamine Purity 99.9% Shanghai Annuo Aromatic Amine Chemicals Co., Ltd. Trimesoyl chloride Purity>97.5% Qingdao Sanlibennuo New Materials Co., Ltd. ISOPAR-G Isoparaffin Boiling range 161-173℃ ExxonMobil 1-Aminoindene-1-carboxylic acid Purity 95% Fluorochem 2-Aminoindene-2-carboxylic acid Purity 95% Fluorochem 2-Naphthoyl chloride Purity 98% Sigma-Aldrich (Shanghai) Trading Co., Ltd. Sodium hypochlorite Purity ≥6% Wanhua Chlor-Alkali Co., Ltd. glycerin Purity 99.5% Shandong Luliya New Materials Co., Ltd. Sodium chloride Purity 99.5% Beijing Inotech Technology Co., Ltd. BSA Purity 98% Sigma-Aldrich (Shanghai) Trading Co., Ltd. Humic acid 100% purity Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0051] Performance testing method:

[0052] Salt rejection rate and permeate flux are two important parameters for evaluating the separation performance of reverse osmosis membranes.

[0053] The desalination rate (R) is defined as: under certain operating conditions, the salt concentration of the feed solution (C f ) and the salt concentration in the permeate (C p ) and then divided by the feed solution salt concentration (C f ), as shown in formula (1).

[0054]

[0055] Permeation flux is defined as the volume of water that passes through a unit membrane area per unit time under certain operating conditions, and its unit is L / (m 2 h).

[0056] The test operation conditions and operation steps adopted in the example are as follows:

[0057] 1. Test the water flux F1 and desalination R1 of 2000ppm sodium chloride solution of the membrane at 1.55MPa;

[0058] 2. The flux was tested after running for 24 hours at 1.55 MPa with a mixed solution of 2000 ppm sodium chloride, 1% bovine serum albumin and 1% humic acid (temperature 25°C);

[0059] 3. Rinse with deionized water, measure the water flux F2 and desalination rate R2 of 2000ppm sodium chloride solution, calculate the flux recovery rate RF [RF = (F2 / F1) * 100%)], which characterizes the anti-pollution performance of the membrane. The higher the flux recovery rate, the better the anti-pollution performance.

[0060] Example 1

[0061] 1) adding 0.5% of 1-aminoindene-1-carboxylic acid and 0.05% of 2-naphthoyl chloride to 3wt% of m-phenylenediamine aqueous solution and 0.25wt% of trimesoyl chloride ISOPAR-G, respectively, and stirring to obtain an aqueous phase solution and an oil phase solution;

[0062] 2) The polysulfone-based membrane is contacted with the aqueous solution for 30 seconds, and an interfacial polymerization reaction begins to occur after contact with the oil phase to form a modified polyamide separation layer, thereby obtaining a basic large-flux anti-fouling reverse osmosis membrane; 3) The basic large-flux anti-fouling reverse osmosis membrane is immersed in a water tank with a pH of 8 and containing 1200ppm sodium hypochlorite for post-treatment for 2 minutes, and then enters a 5% glycerol moisturizing water tank for treatment, and is dried at 70°C for 2 minutes before being rolled up.

[0063] Embodiments 2 to 16

[0064] The high flux reverse osmosis membrane was prepared by the preparation process in Example 1, except that different mass concentrations of indene compounds were added to the aqueous solution and different mass concentrations of 2-naphthoyl chloride were added to the organic solution, and the interfacial polymerization time was also added. The types of additives and the concentrations added are shown in Table 2.

[0065] Comparative Examples 1 to 3

[0066] The reverse osmosis membranes in Comparative Examples 1 to 3 were prepared respectively according to the method substantially the same as that in Example 1, with the only difference being the type of additives and the added concentration as shown in Table 2.

[0067] Table 2 Reaction raw material formula table of embodiment and comparative example

[0068]

[0069] The reverse osmosis membranes prepared in the examples and comparative examples were tested for salt rejection rate R1, flux F1, flux recovery rate RF, Zeta potential test, and composite reverse osmosis membrane polyamide thickness test, and the results are recorded in Table 3 Reverse osmosis membrane performance.

[0070] Table 3 Reverse osmosis membrane performance test data table

[0071]

[0072]

[0073] It can be seen from the experimental results in Table 3 that the addition of indene compounds and 2-naphthoyl chloride containing amino and carboxyl structures forms an interlocking structure with the bulk polymer during the interfacial polymerization process, reorganizes the molecular network structure, cross-links the membrane layers, and greatly improves the interception capacity of the membrane while increasing the membrane thickness. The carboxylic acid groups contained therein increase the hydrophilicity of the membrane surface, which is conducive to the formation of a water layer on the membrane surface and the faster speed of water transporting through the channel in the membrane. The formation of the surface water layer makes it difficult for pollutants to deposit on the membrane surface, which plays an anti-pollution role. The faster speed of water transporting through the channel in the membrane leads to a greater flux of the reverse osmosis membrane. Therefore, the addition of indene compounds and 2-naphthoyl chloride containing amino and carboxyl structures in the reverse osmosis membrane preparation process can not only make the prepared reverse osmosis membrane have a larger flux and a higher desalination rate, but also effectively improve the anti-pollution performance of the reverse osmosis membrane, greatly enhancing the comprehensive performance of the reverse osmosis membrane.

[0074] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A method for preparing a high-flux, anti-pollution reverse osmosis membrane, characterized in that: The following steps are involved: 1) adding an indene compound containing an amino group and a carboxyl group structure to an aqueous solution containing m-phenylenediamine, and stirring the mixture to obtain an aqueous phase solution; adding 2-naphthoyl chloride to an organic phase containing trimesoyl chloride, and stirring the mixture to obtain an oil phase solution; 2) contacting the polysulfone-based membrane with the aqueous solution and the oily solution respectively, causing interfacial polymerization to form a modified polyamide separation layer, thereby obtaining a basic reverse osmosis membrane; 3) The basic reverse osmosis membrane is immersed in a sodium hypochlorite water tank for post-treatment, moisturizing treatment and drying to obtain the high-flux, anti-pollution reverse osmosis membrane.

2. The preparation method according to claim 1, characterized in that: The aqueous phase solution in step 1) contains 0.1-2.0 wt% of indene compounds containing amino and carboxyl structures.

3. The preparation method according to claim 2, characterized in that: The mass concentration of the indene compound containing amino and carboxyl structures in the aqueous phase solution is 0.5% to 1.0%.

4. The preparation method according to claim 3, characterized in that: The indene compound containing amino and carboxyl structures is selected from one or both of 1-aminoindene-1-carboxylic acid and 2-aminoindene-2-carboxylic acid.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In the aqueous solution of step 1), the mass percentage of m-phenylenediamine is 1.5-5.0wt%.

6. The preparation method according to claim 1, characterized in that: The mass concentration of 2-naphthoyl chloride in the oil phase solution of step 1) is 0.02-0.2wt%.

7. The preparation method according to claim 6, characterized in that: The mass concentration of 2-naphthoyl chloride in the oil phase solution of step 1) is 0.05-0.1wt%.

8. The preparation method according to claim 1 or 6, characterized in that: The mass concentration of trimesoyl chloride in the oil phase solution of step 1) is 0.1-0.3wt%.

9. The preparation method according to claim 1, characterized in that: In step 2), the contact time between the polysulfone-based membrane and the aqueous solution is 10s-120s.

10. The preparation method according to claim 9, characterized in that: In step 2), the contact time between the polysulfone-based membrane and the aqueous solution is 30-60 seconds.

11. The preparation method according to claim 10, characterized in that: The interfacial polymerization reaction time in step 2) is 2-60s.

12. The preparation method according to claim 11, characterized in that: The interfacial polymerization reaction time in step 2) is 10-30s.

13. The preparation method according to claim 1, characterized in that: The concentration of the sodium hypochlorite solution in the post-treatment water tank in step 3) is 50-500 ppm.

14. The preparation method according to claim 13, characterized in that: The pH of the sodium hypochlorite solution in the tank is 3-10.

15. The preparation method according to claim 1, characterized in that: In step 3), glycerin or citric acid is used as a moisturizer in the moisturizing treatment.

16. The preparation method according to claim 15, characterized in that: The mass concentration of the moisturizing agent is 1%-20wt%.

17. The preparation method according to claim 15, characterized in that: The drying temperature is 60-90°C and the drying time is 30-180s.

18. A high-flux, anti-fouling reverse osmosis membrane prepared by the preparation method according to any one of claims 1 to 17.

19. Use of a high-flux, anti-fouling reverse osmosis membrane obtained by the preparation method according to any one of claims 1 to 17 or according to claim 18 in separation membranes or water treatment.