Hydrotreating catalyst and its preparation method and application

By impregnating the alumina carrier with Group VIII and VIB metal precursors and other compounds, a catalyst with bimodal pore distribution is formed, which solves the problems of diesel hydrogenation catalyst stability and preparation complexity and achieves high activity and stability. , meeting the hydrodesulfurization and dearomatization reaction efficiency of National VI diesel standards.

CN116037177BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111265080.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-10-15
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Existing diesel hydrogenation catalysts have problems with poor stability and complex preparation processes under the National VI standards, making it difficult to meet the needs for high activity and stability.

Method used

The impregnation method is used to introduce Group VIII metal precursors, VIB Group metal precursors, phosphorus-containing compounds, organic alcohol compounds and carboxylic acid compounds into alumina to form a catalyst with bimodal pore distribution and increase the active metal loading and pore structure. , simplifying the preparation process.

Benefits of technology

It achieves high activity and stability of the catalyst, significantly improves the efficiency of hydrodesulfurization and dearomatization reactions, meets the quality standards of National VI diesel, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of preparation of hydrorefining catalysts, and discloses a hydrorefining catalyst and a preparation method and application thereof. A hydrorefining catalyst, wherein the catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore volume of the catalyst is 0.2-0.4 cm 3 / g, with an average pore size of 6-18nm, wherein the pore size of the catalyst presents a bimodal pore distribution within the range of 2-6nm and 8-20nm. The hydrorefining catalyst has the advantages of good stability, high activity and simple preparation process, and the hydrorefining catalyst is applied to diesel to achieve excellent desulfurization and dearomatization effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogenation catalyst preparation, and in particular to a hydrogenation refining catalyst and a preparation method and application thereof. Background Art

[0002] In the past five years, as the society's environmental awareness continues to increase, the quality standards of clean fuels in my country have shown an accelerated upgrading trend. The diesel quality standard has rapidly moved from National IV and National V to National VI, requiring the sulfur content and polycyclic aromatic hydrocarbons in diesel to be reduced to 10 mg / kg and 7% respectively, and polycyclic aromatic hydrocarbons will tend to be further reduced in the future. This has brought severe challenges to the selection of refinery diesel hydrogenation catalysts and the operation of the unit. Although the product quality can be qualified by increasing the reaction temperature of the unit, it will lead to a significant increase in the catalyst deactivation rate, and at the same time cause the reactor outlet temperature to approach the aromatics thermodynamic equilibrium zone faster, suppressing the polycyclic aromatic hydrocarbons saturation reaction, and greatly shortening the catalyst life cycle. The existing diesel hydrogenation catalyst technology is facing a bottleneck, and it is urgent to develop a diesel hydrogenation catalyst with high activity and high stability.

[0003] The active metals in diesel hydrodesulfurization catalysts are mainly composed of VIB group metals (Mo and / or W) and VIII group metals (Co and / or Ni). In the catalyst, the active metals are highly dispersed on the surface of the carrier to form a large number of active centers. Generally, the hydrogenation catalyst contains a certain pore structure, and during the reaction process, the reactants contact the active centers through the pores of the catalyst to react. Therefore, the diesel hydrogenation catalyst should not only have a large number of active centers, but also the active centers should have good accessibility.

[0004] A Chinese patent application with application number 202010395989.6 discloses a hydrorefining catalyst and its preparation method and application. The catalyst includes 50-80wt% of a carrier and 20-50wt% of an active metal component. The carrier uses a composite oxide to regulate the interaction force between the active metal and the carrier in the catalyst, thereby increasing the concentration of active hydrogen species on the active metal surface and improving the hydrodesulfurization and hydrodenitrogenation reaction activity of the catalyst.

[0005] Chinese patent application No. 201811455219.5 discloses a method for preparing a supported hydrogenation catalyst, wherein one or more of the group consisting of sodium ethylenediaminetetramethylenephosphate, tetrabutylammonium fluoride and tartaric acid are used as active metal positioning loading directing agents, and a γ-Al2O3 carrier is contacted with a solution containing the active metal positioning loading directing agent to prepare a catalyst, wherein the catalyst has high hydrodesulfurization, denitrogenation activity and aromatic saturation activity.

[0006] The Chinese patent application with application number 201711023399.5 discloses a diesel hydrorefining catalyst, comprising 1-30% TS-1 molecular sieve, 20-50% γ-Al2O3, 0.01-10% zirconium oxide, 0.01-5% graphene, 10-40% heteropoly acid calculated as metal oxide, and the catalyst specific surface area is 250-500m 2 / g, pore volume 0.5-0.8mL / g. The catalyst has high hydrodesulfurization activity.

[0007] Chinese patent application No. 201710984468.2 discloses a bulk hydrorefining catalyst, comprising metal components of W, Ni and Mo. The preparation steps of the catalyst include 1) conducting a gelling reaction of a mixed solution A containing Ni, W and Al, an organic additive and a precipitant in parallel, and aging the resulting slurry; 2) then adding a mixed solution B containing W and Al, a MoO3 slurry and a precipitant in parallel to the aged slurry, and then aging; 3) drying, molding and other steps; the catalyst has high hydrodesulfurization and hydrodenitrogenation reaction activity, especially for treating diesel feedstocks with high nitrogen and high sulfur content.

[0008] Chinese patent application with application number 201610542732.2 discloses a hydrogenation catalyst, which is composed of γ-Al2O3 loaded with Co, Ni, W / Mo active components, and contains F as an auxiliary agent. The F-containing compound is at least one of the group consisting of tetrabutylammonium fluoride, trifluoroacetic acid, hexafluoroacetone and hexafluoroisopropanol, and has high hydrodesulfurization activity and aromatic saturation activity.

[0009] Chinese patent application No. 201610388357.0 discloses a hydrodesulfurization catalyst, which includes a composite carrier of NiO, MoO3 and WO3 as well as AlOOH and TiO2. It is a slurry catalyst with high reaction activity and good stability synthesized by a complete liquid phase method, which can meet the needs of ultra-deep hydrodesulfurization of diesel.

[0010] From the above, it can be seen that the research and invention of diesel hydrodesulfurization catalysts have improved the properties of catalysts from many angles, and significantly improved the activity of diesel hydrodesulfurization catalysts. The preparation processes of these inventions are relatively complicated, and their implementation costs and convenience are still insufficient. The stability of the catalysts cannot fully meet the needs of National VI diesel production. Summary of the invention

[0011] The purpose of the present invention is to overcome the problems of poor stability and complicated preparation process of the hydrotreating catalyst in the prior art, and to provide a hydrotreating catalyst and its preparation method and application, which has the advantages of good stability, high activity and simple preparation process.

[0012] In order to achieve the above object, the present invention provides a hydrotreating catalyst in the first aspect, wherein the catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore volume of the catalyst is 0.2-0.4 cm 3 / g, and an average pore size of 6-18nm, wherein the pore size of the catalyst is in the range of 2-6nm and 8-20nm and presents a bimodal pore distribution.

[0013] Preferably, in the catalyst, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for 8-15%, preferably 9-12% of the total pore volume of the catalyst.

[0014] The second aspect of the present invention provides a method for preparing the hydrotreating catalyst according to the first aspect, the method comprising:

[0015] The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina by an impregnation method, and then dried.

[0016] The third aspect of the present invention provides use of the hydrotreating catalyst described in the first aspect in a hydrodesulfurization reaction.

[0017] The inventors found in the study that the hydrorefining catalyst is composed of a carrier and an active metal component (the active metal component in the present invention includes a metal element of Group VIII and a metal element of Group VIB), and the active metal component is dispersed on the surface of the carrier. The carrier required in the catalyst has a pore structure of varying sizes, and the reactant molecules need to pass smoothly through the contact active center during the reaction. An effective way to improve the activity of the hydrorefining catalyst is to increase the content of the active metal component in the catalyst, thereby increasing the number of active centers of the catalyst. The distribution of the active metal component on the surface of the carrier will cause the pore size to shrink, and the stacking height of the active metal on the surface of the carrier will increase when the metal loading is increased. If the metal loading is too high, the active metal will make the pores of the carrier very narrow, and the passage of the reactant molecules will be blocked. If the metal loading is low, the pore space of the catalyst will not be fully utilized, and the role of the carrier pore space cannot be maximized. The present invention achieves the purpose of increasing the active metal loading and making full use of the active components by selecting a carrier with a suitable pore structure and loading an active metal component with an appropriate stacking height on the surface of the carrier.

[0018] The catalyst provided by the present invention has the advantage of a simple preparation method and has good stability and desulfurization activity when used in a hydrodesulfurization reaction process. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] The first aspect of the present invention provides a hydrotreating catalyst, wherein the catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore volume of the catalyst is 0.2-0.4 cm 3 / g, and an average pore size of 6-18nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the ranges of 2-6nm and 8-20nm.

[0021] In the present invention, the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm, which means that the pore size distribution of the catalyst has two peaks in the pore size range of 2-6nm and 8-20nm. Generally, the carrier also has a certain number of pore size distributions in the range of 2-6nm, but this part of the pores of the carrier does not have a peak, and no bimodal pores are formed.

[0022] In the present invention, preferably, in the catalyst, the volume of pores with a pore size distribution of 2-6 nm accounts for 8-15% of the total volume of the catalyst, and more preferably 9-12%. By adopting this preferred embodiment, the effect of the active metal components in the smaller pores and the larger pores can be fully exerted, the reaction efficiency of the catalyst for sulfur-containing compounds of different sizes can be improved, and the purpose of fully utilizing the active metal can be achieved.

[0023] In a preferred embodiment, the specific surface area of ​​the catalyst is 130-170 m 2 / g.

[0024] In a preferred embodiment, the average pore size of the catalyst is 8-10 nm.

[0025] In a preferred embodiment, the pore volume of the catalyst is 0.25-0.4 cm 3 / g.

[0026] Generally, the pores of hydrotreating catalysts are concentrated at 6-20nm. There are reactant molecules of different sizes in diesel feedstock, and larger reaction channels are wider for smaller reactant molecules. The pore size of 2-6nm can provide a good reaction space for smaller reactant molecules, improve the utilization efficiency of the pores inside the catalyst, and achieve the purpose of improving activity. This part of the pores comes from the loaded active metal components, which can promote the synergistic effect of the active centers of the pore wall, thereby better promoting the hydrodesulfurization and aromatic saturation reactions.

[0027] Due to the loading of appropriate active metal components (metal elements of Group VIII and metal elements of Group VIB), the pores of the catalyst present a bimodal pore distribution, with a portion of the pores concentrated at the position where the pore diameter is concentrated in the carrier, and another portion concentrated at 2-6 nm. Due to the loading of the active metal components, pores at 2-6 nm are generated. This bimodal pore diameter structure can meet the requirements of the reaction molecules to diffuse to the active center, and can load sufficient active metal components, so that the performance of the hydrorefining catalyst is greatly improved.

[0028] The hydrorefining catalyst provided by the present invention contains a specific bimodal pore structure. The hydrorefining catalyst is applied to desulfurization and dearomatization of diesel. The hydrorefining catalyst has good stability and excellent desulfurization and dearomatization performance.

[0029] In the present invention, the determination of the specific surface area, pore volume, pore distribution and average pore diameter of the hydrotreating catalyst refers to the determination after the catalyst is calcined at 400° C. for 3 hours.

[0030] In the present invention, the specific surface area, pore distribution, average pore diameter and pore volume of the catalyst are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100 nm is calculated according to the results of BET.

[0031] In the present invention, unless otherwise specified, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.

[0032] In the present invention, in order to meet the performance of the catalyst, a suitable carrier is selected as the catalyst carrier. The type of the carrier is not specifically limited in the present invention and can be obtained commercially. Preferably, the water absorption rate of the alumina is greater than 0.9 mL / g, preferably 0.9-1.2 mL / g.

[0033] Preferably, the specific surface area of ​​the alumina is greater than 260 m 2 / g, preferably 260-400m 2 / g.

[0034] Preferably, the average pore size of the aluminum oxide is greater than 8 nm, more preferably 8-14 nm, and the pore distribution is a unimodal pore distribution. The advantage of adopting this preferred embodiment is that it can ensure sufficient pore space, on the one hand, a certain number of pores with a diameter of 2-6 nm can be formed, and on the other hand, the effects of all active metal components can be exerted.

[0035] In a preferred embodiment, in the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina, more preferably no more than 8%, and more preferably 5-8%.

[0036] In a particularly preferred case, in the alumina, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4% of the total volume of the alumina, and more preferably no more than 2%.

[0037] The use of the above-mentioned preferred carrier is more conducive to improving the utilization of active metals, allowing the active metal components to better enter larger pores, and no pore blockage occurs when the metal loading is high.

[0038] According to a preferred embodiment of the present invention, the catalyst further contains P2O5.

[0039] In the present invention, in order to make the active metal components loaded in the carrier pores, the pores of the catalyst are more reasonably utilized. Preferably, the catalyst composition is as follows: (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, preferably 0.5-0.8nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup The advantage of adopting this preferred embodiment is that it can ensure that a better bimodal pore structure is formed inside the catalyst, so that part of the pores are concentrated in 2-6nm.

[0040] In the present invention, ρMoO3, ρWO3, ρNiO, ρCoO, and ρP2O5 are 4.69 g / cm3 , 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.

[0041] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co, Ni, Ru, Pt and Pd, preferably Co and / or Ni.

[0042] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.

[0043] In the present invention, there is no specific limitation on the amount of P2O5 and the VIB group metal oxide in the catalyst, as long as the performance of the catalyst is improved. Preferably, the molar ratio of Zi / Xi in the catalyst is 0.05-0.3, and more preferably 0.08-0.2. The advantage of adopting this preferred embodiment is that by adopting this metal combination mode, each metal component can better play a synergistic effect with each other, thereby optimizing the activity of the catalyst.

[0044] In a preferred embodiment, in order to further improve the performance of the catalyst, the atomic concentration of the VIB group metal element in the catalyst on the carrier surface is 5-13 atom / nm 2 , preferably 5-11atom / nm 2 The advantage of adopting this preferred embodiment is that the amount of active metal is relatively moderate, which can promote the generation of pores with a diameter of 2-6 nm.

[0045] In the present invention, the atomic concentration of the VIB group metal element on the carrier surface refers to the average atomic concentration of the VIB group metal element on the carrier surface, which is obtained by measuring the metal loading and the specific surface area of ​​the carrier and then calculating. Specifically, it can be calculated as follows: atomic concentration = (ai / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of carrier Xi, M Xi is the molecular weight of Xi, SA sup is the specific surface area of ​​the carrier.

[0046] In a preferred embodiment, the atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.05-0.35, preferably 0.1-0.3.

[0047] In the present invention, preferably, the catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the metal elements of Group VIII is 1 to 6, preferably 2 to 5. The purpose of adopting this preferred embodiment is to ensure that the metal elements of Group VIII have a higher dispersibility, weaken the interaction between the carrier and the metal, and promote the generation of more active phases.

[0048] The organic alcohol compound containing -OH can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a preferred case, the organic alcohol compound containing -OH is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane, preferably at least one of glycerol, propanol and ethylene glycol.

[0049] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, preferably at least one of formic acid, citric acid and acetic acid.

[0050] In a particularly preferred embodiment, the catalyst further comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.

[0051] In the present invention, the size of the catalyst can be selected from a wide range, and those skilled in the art can make an appropriate selection according to the specific application of the catalyst. Preferably, the equivalent diameter of the catalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm.

[0052] In the present invention, there is no specific limitation on the shape of the catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, clover, four-leaf clover, butterfly, honeycomb or other irregular shapes, more preferably butterfly.

[0053] The present invention has no particular limitation on the method for preparing the above catalyst, and any method that can prepare the catalyst with the above composition and structure can be used in the present invention.

[0054] The second aspect of the present invention provides a method for preparing the hydrotreating catalyst according to the first aspect, the method comprising:

[0055] The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina by an impregnation method, and then dried.

[0056] In the present invention, the "optionally containing -OH organic alcohol compounds and / or carboxylic acid compounds" means that -OH-containing organic alcohol compounds and / or carboxylic acid compounds may be introduced into alumina, or may not be introduced, but introduction is preferred.

[0057] In the present invention, the types of Group VIII metals, Group VIB metals, -OH-containing organic alcohol compounds, and carboxylic acid compounds have been described in the first aspect and will not be elaborated on here.

[0058] In the present invention, the metal element species in the VIB group metal oxide and the VIII group metal oxide are provided by a precursor containing the above metal elements. Preferably, the VIB group metal precursor is selected from at least one of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.

[0059] In a preferred embodiment, the Group VIII metal precursor is at least one selected from cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.

[0060] In a particularly preferred embodiment, the VIB Group metal and VIII Group metal precursor is selected from at least one of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate, tungsten oxide, cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.

[0061] In the present invention, P2O5 is provided by a phosphorus-containing compound. Preferably, the phosphorus-containing compound is selected from at least one of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.

[0062] In the present invention, preferably, the amounts of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound are such that the catalyst obtained satisfies the above (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value required.

[0063] According to the method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. It can be co-impregnation, step-by-step impregnation, saturation impregnation, or supersaturation impregnation. Preferably, co-impregnation is adopted. Preferably, the impregnation method comprises: impregnating the aluminum oxide with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.

[0064] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and the optionally -OH-containing organic alcohol compound and / or carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the -OH-containing organic alcohol compound and / or carboxylic acid compound, the Group VIII metal precursor, and the Group VIB metal precursor are added to an aqueous solution of the phosphorus-containing compound to provide the impregnation solution. The order of adding the -OH-containing organic alcohol compound and / or carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.

[0065] According to the method provided by the present invention, the prepared catalyst can have the structure and composition of the first aspect described above according to the physical properties of the carrier and the amount of each material. The present invention has no particular limitation on this. In order to fully illustrate the technical solution of the present invention and facilitate understanding, an exemplary description of the method provided by the present invention is now provided, and the present invention is not limited thereto. For example, a hydrotreating catalyst can be prepared by the following preparation method: (1) Determine the amount of the Group VIB metal precursor per gram of carrier according to the atomic concentration of the Group VIB metal element and the specific surface area of ​​the carrier (alumina); (2) Determine the amount of the Group VIII metal precursor per gram of carrier according to the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element; (3) Determine the amount of the Group VIII metal precursor per gram of carrier according to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA supThe content of P2O5 is calculated based on the value of , and then the amount of phosphorus-containing compound per gram of carrier is determined; (4) the amount of organic alcohol compound and / or carboxylic acid compound containing -OH is calculated based on the molar ratio of organic alcohol compound and / or carboxylic acid compound containing -OH to metal element of Group VIII; (5) according to the feed amounts of Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound containing -OH, alumina is impregnated with impregnation solution by pore saturation impregnation method, and then dried. Specifically, the phosphorus-containing compound is first dissolved in water, and then an organic alcohol compound and / or a carboxylic acid compound containing -OH, a Group VIB metal precursor and a Group VIII metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is kept constant to obtain an impregnation solution; (6) the water absorption rate of the carrier is measured, and the liquid absorption rate of the carrier is calculated according to the formula of carrier water absorption rate-0.1; (7) according to the liquid absorption rate of the carrier, the impregnation solution is adjusted to a corresponding volume (carrier liquid absorption rate×carrier mass), and the impregnation solution and the corresponding mass of the carrier are evenly mixed and allowed to stand, and then dried to prepare a catalyst.

[0066] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.

[0067] The third aspect of the present invention provides use of the hydrotreating catalyst described in the first aspect in a hydrodesulfurization reaction.

[0068] In the present invention, the hydrotreating catalyst is used for distillate oil hydrodesulfurization. Preferably, the sulfur content in the distillate oil to be treated is 5000-30000 ppm, and the aromatic content is 20-80% by weight.

[0069] In a preferred case, the catalyst needs to be converted from an oxidized catalyst to a sulfurized catalyst by sulfurization before use. In the present invention, there is no specific limitation on the sulfurization method, and conventional sulfurization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry sulfurization and wet sulfurization. There is no particular limitation on the type of the vulcanizing agent, and it can be selected according to conventional schemes in the art.

[0070] Preferably, the vulcanization conditions include: vulcanization temperature of 280-420°C, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1, and the preferred heating rate is 5-60°C / hour.

[0071] In a preferred embodiment, the hydrodesulfurization conditions include: pressure of 5-15 MPa, temperature of 260-410°C, volume space velocity of 0.5-10 hours-1 , the volume ratio of hydrogen to oil is 200-1000:1.

[0072] The present invention will be described in detail below by way of examples. In the following examples, the hydrodesulfurization performance of the catalyst was measured on a 20 mL high pressure microreactor, and the oxidized catalyst was directly converted into a sulfurized catalyst by a programmed temperature sulfurization method. The sulfurization conditions were: the sulfurization pressure was 6.4 MPa, the sulfurized oil was kerosene containing 2 wt% CS2, and the volume space velocity was 2 hours. -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then heat it up to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test. The reaction raw materials have a sulfur content of 10890ppm and an aromatic content of 39.0wt% of high aromatic distillate oil. The test conditions are: pressure of 6.4MPa, volume space velocity of 1.5h -1 , the volume ratio of hydrogen to oil was 300 v / v, and the reaction temperature was 340°C. The properties of the product were analyzed after the reaction was stable for 2 days. In order to examine the stability of the catalyst, the mass fraction of sulfur in the reaction product was kept at 10 ppm, the reaction temperature was adjusted every day, and the operation was continued for 5 days. The changes in the reaction temperature before and after 5 days were compared to measure the stability of the catalyst.

[0073] The composition of the catalyst is calculated based on the feed amount. The specific surface area of ​​2-100 nm, pore distribution, pore diameter and pore volume in the catalyst and the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000), and the content of aromatics is analyzed by near infrared spectroscopy.

[0074] The feeding amount of each material in the following examples is determined according to the specific exemplary description given in the text of the present invention.

[0075] Example 1

[0076] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0077] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0078] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0079] The atomic concentration of Mo in the catalyst is 7atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.29, P2O5 / MoO3 molar ratio is 0.13, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.5 nm, and the molar ratio of glycerol to Ni is 2.

[0080] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 165m 2 / g, pore volume 0.38cm 3 / g, the average pore size is 9.2nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 9.2% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 8ppm and the aromatics content was 23.5%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 3.2℃ after 5 days of reaction.

[0081] Example 2

[0082] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0083] MoO3, basic nickel carbonate and glycerol were added to the phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0084] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0085] The atomic concentration of Mo in the catalyst is 11atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.72 nm, and the molar ratio of glycerol to Ni is 5.

[0086] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 151m 2 / g, pore volume 0.32cm 3 / g, the average pore size is 8.5nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 9% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 4.2ppm and the aromatics content was 22.6%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.8℃ after 5 days of reaction.

[0087] Example 3

[0088] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0089] MoO3, basic nickel carbonate and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 90°C for 3 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0090] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0091] The atomic concentration of Mo in the catalyst is 8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.623 nm, and the molar ratio of glycerol to Ni is 3.

[0092] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 164m 2 / g, pore volume 0.35cm 3 / g, the average pore size is 8.5nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 9.8ppm and the aromatics content was 23.6%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 3.3℃ after 5 days of reaction.

[0093] Example 4

[0094] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of ​​280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0095] Ammonium metatungstate, basic nickel carbonate and citric acid were added to the phosphoric acid aqueous solution respectively, heated and stirred at 90°C for 2 hours until completely dissolved and kept at constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0096] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0097] The atomic concentration of W in the catalyst is 5atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.407 nm, and the molar ratio of citric acid to Ni is 2.

[0098] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 162m 2 / g, pore volume 0.39cm 3 / g, the average pore size is 9.6nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 10.5% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 5.6ppm and the aromatics content was 23.1%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 3.2℃ after 5 days of reaction.

[0099] Example 5

[0100] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0101] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0102] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0103] The atomic concentration of Mo in the catalyst is 9atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.12, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.62 nm, and the molar ratio of citric acid to Ni is 2.

[0104] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 154m 2 / g, pore volume 0.36cm 3 / g, the average pore size is 9.4nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 9.8% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 7.8ppm and the aromatics content was 23.2%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 2.9℃ after 5 days of reaction.

[0105] Example 6

[0106] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of ​​270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.

[0107] MoO3, basic nickel carbonate and citric acid were added to a phosphoric acid aqueous solution, heated and stirred at 95°C for 3 hours until completely dissolved and kept at a constant temperature for 2 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0108] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0109] The atomic concentration of Mo in the catalyst is 10atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.27, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.85 nm, and the molar ratio of citric acid to Ni is 2.

[0110] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 135m 2 / g, pore volume 0.27cm 3 / g, the average pore size is 8.0nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 12.5% ​​of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 8.6ppm and the aromatics content was 23.2%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 3.1℃ after 5 days of reaction.

[0111] Comparative Example 1

[0112] The same carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0113] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0114] The atomic concentration of Mo in the catalyst is 4atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.22, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.34nm, and the molar ratio of propylene glycol and Ni is 2.

[0115] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 205m 2 / g, pore volume 0.48cm 3 / g, the average pore size is 9.5nm, the pore size distribution of the catalyst is a single peak pore, and the position of the single peak pore is 8.9nm. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 32ppm and the aromatics content is 27.2%. When the sulfur content of the product is kept at 10ppm, the reaction temperature increases by 4.3℃ after 5 days of reaction.

[0116] Comparative Example 2

[0117] The same carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to a phosphoric acid aqueous solution, stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.

[0118] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0119] The atomic concentration of Mo in the catalyst is 15atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 1.13 nm, and the molar ratio of glycerol to Ni is 2.

[0120] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 118m 2 / g, pore volume 0.19cm 3 / g, the average pore size is 6.4nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 14.0% of the total pore volume. After the catalyst was sulfurized and reacted, the sulfur content in the product was 46ppm and the aromatics content was 28.2%. When the sulfur content of the product was kept at 10ppm, the reaction temperature increased by 4.7℃ after 5 days of reaction.

[0121] Comparative Example 3

[0122] The same carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to a phosphoric acid aqueous solution, heated and stirred at 85°C for 2 hours until completely dissolved and kept at a constant temperature for 3 hours to obtain an impregnation solution containing active metal components. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours. After drying at 120°C for 5 hours, a catalyst with a particle size of 1.6 mm and a butterfly shape was prepared.

[0123] The amount of the carrier and each component is such that the prepared catalyst satisfies:

[0124] The atomic concentration of Mo in the catalyst is 5.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.15, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.35 nm, and the molar ratio of glycerol to Ni is 2.

[0125] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of ​​the catalyst is 186m 2 / g, pore volume 0.46cm 3 / g, the average pore size is 9.9nm, the pore structure shows a single peak pore distribution characteristic, and the position of the single peak pore is 8.6nm. After the catalyst is sulfurized and reacted, the sulfur content in the product is 38ppm and the aromatics content is 27.9%. When the sulfur content of the product is kept at 10ppm, the reaction temperature increases by 4.2℃ after 5 days of reaction.

[0126] It can be seen from the data of the examples and comparative examples that the present invention has a good effect, the prepared hydrotreating catalyst has high activity and stability, and has excellent desulfurization and dearomatization performance in distillate oil.

[0127] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A hydrotreating catalyst, wherein: The catalyst comprises at least one metal element of Group VIII, at least one metal element of Group VIB and alumina, and the pore volume of the catalyst is 0.2-0.4 cm 3 / g, with an average pore size of 6-18nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; In the catalyst, the pore volume with a pore size distribution of 2-6 nm accounts for 8-15% of the total pore volume of the catalyst; The specific surface area of ​​the catalyst is 130-170m 2 / g.

2. The catalyst according to claim 1, wherein In the catalyst, the pore volume with pore size distribution between 2-6 nm accounts for 9-12% of the total pore volume of the catalyst.

3. The catalyst according to claim 1, wherein The average pore size of the catalyst is 8-10 nm.

4. The catalyst according to claim 1, wherein The pore volume of the catalyst is 0.25-0.4 cm 3 / g.

5. The catalyst according to claim 1, wherein The water absorption rate of the alumina is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, the average pore size is greater than 8nm, and the pore distribution morphology is a unimodal pore distribution.

6. The catalyst according to claim 1, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina.

7. The catalyst according to claim 6, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 8% of the total pore volume of the alumina.

8. The catalyst according to claim 1, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4% of the total pore volume of the alumina.

9. The catalyst according to claim 8, wherein In the alumina, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 2% of the total pore volume of the alumina.

10. The catalyst according to any one of claims 1 to 9, wherein Catalyst composition according to (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, where Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-0.9nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of ​​the carrier.

11. The catalyst according to claim 10, wherein The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.5-0.8nm.

12. The catalyst according to claim 10, wherein The molar ratio of Zi / Xi in the catalyst is 0.05-0.

3.

13. The catalyst according to claim 12, wherein The molar ratio of Zi / Xi in the catalyst is 0.08-0.

2.

14. The catalyst according to any one of claims 1 to 9, wherein The atomic concentration of the VIB group metal elements in the catalyst on the carrier surface is 5-13atom / nm 2 .

15. The catalyst according to claim 14, wherein The atomic concentration of the VIB group metal elements in the catalyst on the carrier surface is 5-11atom / nm 2 .

16. The catalyst according to any one of claims 1 to 9, wherein The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.05-0.

35.

17. The catalyst according to claim 16, wherein The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.1-0.

3.

18. The catalyst according to any one of claims 1 to 9, wherein The catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the metal element of Group VIII is 1-6.

19. The catalyst according to claim 18, wherein The molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 2-5.

20. The catalyst according to any one of claims 1 to 9, wherein The equivalent diameter of the catalyst is 0.5-1.8 mm.

21. The catalyst according to claim 20, wherein The equivalent diameter of the catalyst is 0.8-1.6 mm.

22. The catalyst according to any one of claims 1 to 9, wherein The catalyst is in the shape of a cylinder, a three-leaf clover, a four-leaf clover, a butterfly, a honeycomb or other irregular shapes.

23. A method for preparing a hydrotreating catalyst according to any one of claims 1 to 22, comprising: The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina by an impregnation method, and then dried.

24. The preparation method according to claim 23, wherein: The impregnation method comprises: impregnating the aluminum oxide with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.

25. The preparation method according to claim 24, wherein: The -OH-containing organic alcohol compound and / or carboxylic acid compound, Group VIII metal precursor, and Group VIB metal precursor are added to an aqueous solution of a phosphorus-containing compound to provide the impregnation solution.

26. The preparation method according to claim 23, wherein The drying conditions include: temperature of 80-200° C. and time of 1-10 h.

27. Use of the hydrotreating catalyst according to any one of claims 1 to 22 in a hydrodesulfurization reaction.