Hydrodenitrogenation catalyst and its preparation method and application
By combining a modified alumina carrier with Group VIII and VIB metals, a hydrodenitrification catalyst with a bimodal pore structure is prepared, which solves the problem of insufficient activity of the existing catalyst, achieves efficient diesel denitrification effect and reduces the preparation cost.
Patent Information
- Application Number
- CN202111266375.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing diesel hydrodenitrification catalysts have insufficient activity and cannot fully meet the demand for diesel denitrification reactions in conventional cycles. Moreover, the preparation process is complex and the cost is high.
A combination of modified alumina carrier and Group VIII metal and Group VIB metal elements is used, and metal precursors and weakly acidic components are introduced through the impregnation method to prepare a hydrodenitrification catalyst with a bimodal pore structure and increase the loading of active metals. quantity and dispersion.
The hydrodenitrification performance of the catalyst is significantly improved, and it can effectively treat diesel fractions with high nitrogen content. It has excellent industrial prospects and low implementation costs.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogenation catalysts, and in particular to a hydrogenation denitrogenation catalyst and a preparation method and application thereof. Background Art
[0002] In the past five years, my country's diesel quality standards have rapidly moved from National IV and National V to National VI, requiring the sulfur content and polycyclic aromatic hydrocarbons in diesel to be reduced to 10 mg / kg and 7%, respectively. In addition, the development of new energy will also have an impact on the demand for fossil fuels. The social demand for diesel may be reduced to a certain extent, and the diesel fraction needs to be processed using different processes. Many diesel fractions have a high nitrogen content, and a strong hydrodenitrogenation catalyst is required to remove the nitrogen before the diesel can be subsequently processed. Therefore, the development of high-performance diesel hydrodenitrogenation catalysts is of great significance to the comprehensive utilization of diesel fractions.
[0003] The active metals in diesel hydrodenitrogenation catalysts are mainly composed of VIB group metals (Mo and / or W) and VIII group metals (Co and / or Ni). In the catalyst, the active metals are highly dispersed on the surface of the carrier to form a large number of active centers. Generally, the hydrogenation catalyst contains a certain pore structure, and during the reaction process, the reactants contact the active centers through the pores of the catalyst to react. Therefore, the diesel hydrogenation catalyst should not only have a large number of active centers, but also the active centers should have good accessibility.
[0004] Patent application CN111558377A discloses a hydrorefining catalyst and its preparation method and application. The catalyst includes 50-80wt% of a carrier and 20-50wt% of an active metal component. The carrier uses a composite oxide to regulate the interaction between the active metal and the carrier in the catalyst, thereby increasing the concentration of active hydrogen species on the active metal surface and improving the catalyst's hydrodesulfurization and hydrodenitrogenation reaction activity.
[0005] Patent application CN111250103A discloses a method for preparing a supported hydrogenation catalyst, wherein one or more of the group consisting of ethylenediaminetetramethylene phosphate, tetrabutylammonium fluoride and tartaric acid are used as active metal positioning loading directing agents, and a γ-Al2O3 carrier is contacted with a solution containing the active metal positioning loading directing agent to prepare a catalyst, wherein the catalyst has high hydrodesulfurization, denitrogenation activity and aromatic saturation activity.
[0006] Patent application CN109692712A discloses a bulk hydrorefining catalyst, which contains metal components such as W, Ni and Mo. The preparation steps of the catalyst include 1) conducting a gelling reaction of a mixed solution A containing Ni, W and Al, an organic auxiliary agent and a precipitant in parallel, and aging the resulting slurry; 2) adding a mixed solution B containing W and Al, a MoO3 slurry and a precipitant in parallel to the aged slurry, and then aging; 3) drying, molding and other steps; the catalyst has high hydrodesulfurization and hydrodenitrogenation reaction activity, especially for treating diesel feedstocks with high nitrogen and high sulfur content.
[0007] From the above content, it can be seen that the research and invention of diesel hydrodenitrogenation catalysts have improved the hydrodenitrogenation performance of catalysts from many angles, but the preparation processes of these inventions are relatively complicated, and their implementation costs and convenience still have certain shortcomings. The activity of the catalyst cannot fully meet the needs of regular diesel denitrogenation reactions. Summary of the invention
[0008] The purpose of the present invention is to overcome the problem of low catalyst activity in the prior art and to provide a hydrodenitrogenation catalyst and a preparation method and application thereof. The hydrodenitrogenation catalyst has the advantages of high activity, has an excellent denitrification effect on the treatment of diesel fractions, and can be well applied in industrial production.
[0009] In order to achieve the above object, the present invention provides a hydrodenitrogenation catalyst in a first aspect, wherein the catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier, and the pore volume is 0.15-0.5 cm 3 / g, with an average pore size of 6-15nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; the modified alumina carrier contains a weakly acidic component.
[0010] Preferably, the weakly acidic component is selected from at least one of B, P, Si, F and Ge elements.
[0011] Preferably, in the modified alumina carrier, the content of the weakly acidic component is 0.5-10 wt % calculated as oxide.
[0012] Preferably, in the modified alumina carrier, the B2O3 content is not more than 5 weight%, or the P2O5 content is not more than 6 weight%, or the SiO2 content is not more than 10 weight%, or the F content is not more than 5 weight%, or the GeO2 content is not more than 6 weight%.
[0013] The second aspect of the present invention provides a method for preparing the hydrodenitrogenation catalyst described in the first aspect, the method comprising: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound and optionally an organic alcohol compound and / or a carboxylic acid compound containing -OH into a modified alumina carrier by an impregnation method, and then drying.
[0014] The third aspect of the present invention provides use of the hydrodenitrogenation catalyst described in the first aspect in a hydrodenitrogenation reaction.
[0015] The present invention provides a hydrodenitrification catalyst having a specific bimodal pore structure. During the preparation of the catalyst, a weakly acidic component is used to modify an alumina carrier to obtain a modified alumina carrier, which provides a favorable environment for active metal elements (Group VIII metal elements and Group VIB metal elements) during the loading process, so that the hydrodenitrification catalyst has good activity and excellent denitrification performance for high-nitrogen content distillate oil, and has good industrial prospects. DETAILED DESCRIPTION
[0016] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0017] The first aspect of the present invention provides a hydrodenitrogenation catalyst, wherein the catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier, and the pore volume is 0.15-0.5 cm 3 / g, with an average pore size of 6-15nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; the modified alumina carrier contains a weakly acidic component.
[0018] In the present invention, the denitrification performance of the hydrodenitrification catalyst is improved by increasing the content of the active metal element in the catalyst and increasing the number of active centers of the catalyst. The distribution of the active metal element on the surface of the modified alumina carrier will cause the pore size to shrink, and increasing the loading of the active metal element will increase the stacking height of the active metal element on the surface of the modified alumina carrier. The present invention achieves the purpose of increasing the loading of the active metal element and making full use of the active metal element by selecting a modified alumina carrier with a suitable pore structure and loading the active metal element with a suitable stacking height on the surface of the modified alumina carrier.
[0019] At the same time, in the present invention, a weakly acidic component is introduced into the alumina carrier to modify the alumina carrier to obtain a modified alumina carrier. The introduction of the weakly acidic component can promote the dispersion of active metal elements and promote the hydrogenation and denitrogenation activity of the catalyst, thereby more effectively improving the denitrogenation performance of the catalyst in a limited space.
[0020] In the present invention, the pore size of the catalyst presents bimodal pores in the range of 2-6nm and 8-20nm, which means that the pore size distribution of the catalyst has peaks in the pore size range of 2-6nm and 8-20nm. Generally, the carrier also has a certain number of pore size distributions in the range of 2-6nm, but this part of the pores of the carrier does not have a peak, and no bimodal pores are formed.
[0021] In the present invention, the specific surface area, pore volume, average pore diameter and pore distribution of the denitrogenation hydrogenation catalyst are measured after the catalyst is calcined at 400 degrees for 3 hours.
[0022] In the present invention, the specific surface area, pore volume, average pore size and pore distribution of the denitrogenation hydrogenation catalyst are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100 nm is calculated according to the results of BET.
[0023] In the present invention, unless otherwise specified, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.
[0024] In the present invention, there is no specific limitation on the type of weakly acidic component. Preferably, the weakly acidic component is selected from at least one of B, P, Si, F and Ge; further preferably, the weakly acidic component is selected from at least one of B, P and Si. The advantage of adopting this preferred embodiment is that the introduction of the weakly acidic component promotes the hydrogenation performance of the active component and the breaking ability of the CN bond, thereby promoting the denitrification performance of the hydrodenitrification catalyst.
[0025] In the present invention, there is no specific limitation on the content of the weak acid component, as long as it can meet the performance requirements of the catalyst. Preferably, in the modified alumina carrier, the content of the weak acid component is 0.5-10 wt %, more preferably 1.5-8 wt %, calculated as oxide.
[0026] In the present invention, the weakly acidic component is provided by a compound containing a weakly acidic component. In a preferred embodiment, in the modified alumina carrier, the content of B2O3 is not more than 5 weight%, or the content of P2O5 is not more than 6 weight%, or the content of SiO2 is not more than 10 weight%, or the content of F is not more than 5 weight%, or the content of GeO2 is not more than 6 weight%.
[0027] In a particularly preferred embodiment, the modified alumina carrier has a B2O3 content of 1.5-5% by weight, a P2O5 content of 2-6% by weight, a SiO2 content of 6-10% by weight, a F content of 1-3% by weight, or a GeO2 content of 2-4% by weight.
[0028] In the present invention, there is no specific limitation on the method for introducing the weakly acidic component, and conventional methods in the art are applicable to the present invention. For example, an impregnation method can be selected. In a preferred embodiment, the present invention adopts a co-impregnation method to introduce the weakly acidic component.
[0029] In the present invention, there is no particular restriction on the timing of introducing the weakly acidic component, and the weakly acidic component can be introduced during the preparation of the alumina support or after the preparation of the alumina support. Preferably, the following method can be adopted: the weakly acidic component is introduced after the preparation of the alumina support, and then calcined to obtain a modified alumina support.
[0030] In the present invention, when the weakly acidic component is introduced after the alumina carrier is prepared, the weakly acidic component is provided by a compound containing the weakly acidic component. Preferably, the compound containing the weakly acidic component is selected from at least one of boric acid, silica sol, phosphoric acid, hypophosphorous acid, ammonium phosphate, ammonium dihydrogen phosphate, ammonium fluoride, sodium germanate and germanium hydroxide.
[0031] In the present invention, the specific conditions for calcination can be selected in a wide range. Preferably, the calcination temperature is 500-800°C and the calcination time is 2-10 hours.
[0032] In the present invention, when the weakly acidic component is introduced during the preparation of the alumina carrier, preferably, the compound containing the weakly acidic component can be directly added in the form of a precursor.
[0033] There is no specific limitation on the preparation method of the alumina carrier in the present invention. Conventional preparation methods in the art are applicable to the present invention and will not be described in detail herein.
[0034] In the present invention, a modified alumina carrier having specific physical properties is selected as a carrier of the hydrodenitrogenation catalyst. Preferably, the water absorption rate of the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 250 m 2 / g, the average pore size is greater than 9nm, and further preferably, the water absorption rate of the modified alumina carrier is 0.9-1.1mL / g, the specific surface area is 250-360m 2 / g, average pore diameter 9-14nm, pore distribution morphology is unimodal pore distribution. This preferred implementation can give full play to the effect of active metals in smaller pores and larger pores, improve the reaction efficiency of the catalyst for nitrogen-containing compounds of different sizes, and achieve the purpose of fully utilizing active metals.
[0035] In a preferred embodiment, in the modified alumina carrier, the pore volume with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the modified alumina carrier, more preferably no more than 8%, and further 5-8%.
[0036] In a preferred embodiment, in the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4%, preferably no more than 3% of the total pore volume of the modified alumina carrier.
[0037] The use of the above preferred modified alumina carrier is more conducive to the loading of active components and avoids the formation of agglomerated particles.
[0038] In a preferred embodiment, in the catalyst, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 7-15% of the total pore volume of the catalyst, and more preferably 8-13%.
[0039] In a preferred embodiment, the specific surface area of the catalyst is 110-200m 2 / g, preferably 130-170m 2 / g.
[0040] In a preferred embodiment, the average pore size of the catalyst is 6-12 nm, preferably 6-10 nm.
[0041] In a preferred embodiment, the pore volume of the catalyst is 0.2-0.4 cm 3 / g.
[0042] The present invention provides a hydrodenitrogenation catalyst having the above-mentioned specific structure, which has excellent denitrogenation performance in high-nitrogen fraction oil and has good activity.
[0043] In a preferred embodiment, the catalyst further contains P2O5, where P2O5 refers to P2O5 other than the compound containing P weakly acidic component introduced into the modified alumina carrier.
[0044] In the present invention, in order to better utilize the pores of the catalyst and give full play to the performance of the catalyst. Preferably, the composition of the catalyst is as follows: ai )·(Yibi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass fraction relative to 1 gram of the modified alumina carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass fraction relative to 1 gram of the modified alumina carrier Yi, Zi is P2O5, ci is the mass fraction relative to 1 gram of the modified alumina carrier P2O5, Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-1nm, preferably 0.45-0.85nm, ρ Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the modified alumina support.
[0045] In the present invention, ρMoO3, ρWO3, ρNiO, ρCoO, and ρP2O5 are 4.69 g / cm 3 , 7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.
[0046] It is hereby explained that ci here is the mass of P2O5 relative to 1 gram of modified alumina carrier, and P2O5 refers to P2O5 other than the weakly acidic component P2O5 in the modified alumina carrier, that is, it does not include the weakly acidic component P2O5 in the modified alumina carrier.
[0047] In the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co and Ni, preferably Co and / or Ni.
[0048] In a preferred embodiment, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.
[0049] In the present invention, there is no particular limitation on the amount of P2O5 and the metal oxide of Group VIB. Preferably, the molar ratio of Zi / Xi in the catalyst is 0.1-0.4, more preferably 0.1-0.35. The advantage of adopting this preferred embodiment is that the metal components can better exert the synergistic effect with each other, thereby optimizing the activity of the catalyst.
[0050] In a preferred embodiment, the atomic concentration of the metal element of Group VIB in the catalyst on the surface of the modified alumina carrier is 4.5-14 atom / nm 2 , preferably 5-12atom / nm 2 The advantage of adopting this preferred embodiment is that the amount of active metal is relatively moderate, which can promote the formation of pores with a diameter of 2-6 nm on the one hand, and can promote the overall activity of the hydrodenitrogenation catalyst for hydrodenitrogenation on the other hand.
[0051] In the present invention, the atomic concentration of the VIB group metal element in the catalyst on the surface of the modified alumina carrier refers to the average atomic concentration of the VIB group metal element on the surface of the modified alumina carrier, which is obtained by measuring the metal loading and the specific surface area of the carrier and then calculating. Specifically, it can be obtained by the following calculation: atomic concentration = (a / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of modified alumina carrier Xi, M Xi is the molecular weight of Xi, SA sup is the specific surface area of the carrier.
[0052] In a preferred embodiment, in order to further improve the performance of the catalyst, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the catalyst is 0.1-0.4, preferably 0.2-0.3.
[0053] In this aspect, preferably, the catalyst further comprises one or more -OH-containing organic alcohol compounds and / or carboxylic acid compounds, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the Group VIII metal elements is 1 to 6, preferably 2 to 5. The purpose of adopting this preferred embodiment is to ensure that the Group VIII metal elements have high dispersibility, weaken the interaction between the modified alumina support and the metal, and promote the generation of more active phases.
[0054] In a preferred embodiment, the organic alcohol compound containing -OH can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. In a particularly preferred embodiment, the organic alcohol compound containing -OH is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane. In a more particularly preferred embodiment, the organic alcohol compound containing -OH is selected from at least one of glycerol, propanol and ethylene glycol.
[0055] In a preferred embodiment, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, and is further preferably at least one of formic acid, citric acid and acetic acid.
[0056] In a particularly preferred embodiment, the catalyst comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.
[0057] In the present invention, there is no specific limitation on the size of the catalyst. Preferably, the equivalent diameter of the catalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm.
[0058] In the present invention, there is no specific limitation on the shape of the catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, butterfly, clover, four-leaf clover, honeycomb or other irregular shapes, more preferably cylindrical or butterfly.
[0059] The present invention has no particular limitation on the preparation method of the above catalyst, and any preparation method that can prepare the catalyst with the above composition and structure can be used in the present invention.
[0060] The second aspect of the present invention provides a method for preparing the hydrotreating catalyst according to the first aspect, the method comprising:
[0061] The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the modified alumina carrier by an impregnation method, and then dried.
[0062] In the present invention, the "optionally containing -OH organic alcohol compounds and / or carboxylic acid compounds" means that -OH-containing organic alcohol compounds and / or carboxylic acid compounds may be introduced into the modified alumina carrier, or may not be introduced. In the present invention, introduction is preferred.
[0063] In the present invention, the types of Group VIII metals, Group VIB metals, -OH-containing organic alcohol compounds, and carboxylic acid compounds have been described in the first aspect and will not be elaborated on here.
[0064] In the present invention, the metal element species in the VIB group metal oxide and the VIII group metal oxide are provided by a precursor containing the above metal elements. Preferably, the VIB group metal precursor includes but is not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.
[0065] In a preferred embodiment, the Group VIII metal precursor includes, but is not limited to, one or more of cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0066] In a particularly preferred embodiment, the VIB Group metal and VIII Group metal precursors include but are not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate, tungsten oxide, cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0067] In a preferred embodiment, P2O5 is provided by a phosphorus-containing compound. Further preferably, the phosphorus-containing compound includes but is not limited to one or more of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0068] In a preferred embodiment, the amount of the Group VIII metal precursor, the Group VIB metal precursor, and the phosphorus-containing compound is such that the catalyst obtained satisfies the above (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value required.
[0069] According to the preparation method of the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. For example, it can be one of co-impregnation, step-by-step impregnation, saturated impregnation and supersaturated impregnation. In a preferred embodiment, the present invention adopts a co-impregnation method to prepare the catalyst. In a more preferred embodiment, the impregnation method comprises: impregnating the modified alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
[0070] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and the optionally -OH-containing organic alcohol compound and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the Group VIII metal precursor, the Group VIB metal precursor, and the -OH-containing organic alcohol compound and / or the carboxylic acid compound are added to an aqueous solution of the phosphorus-containing compound to prepare the impregnation solution. In the present invention, the order of adding the -OH-containing organic alcohol compound and / or the carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.
[0071] According to the preparation method provided by the present invention, the prepared catalyst has the structure and composition of the first aspect according to the physical properties of the modified alumina carrier and the amount of each material. The present invention has no particular limitation on this. In order to facilitate the understanding of the technical solution of the present invention, an exemplary description is now provided to embody the preparation method of the present invention, and the method of the present invention includes but is not limited to this. For example, the hydrodenitrogenation catalyst can be prepared by the following preparation method: (1) According to the atomic concentration of the VIB group metal element and the specific surface area of the modified alumina carrier, the feeding amount of the VIB group metal precursor per gram of the modified alumina carrier is determined; (2) According to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element, the feeding amount of the VIII group metal precursor per gram of the modified alumina carrier is determined; (3) According to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA supThe content of P2O5 is calculated based on the value of , and then the amount of phosphorus-containing compound per gram of carrier is determined; (4) the amount of organic alcohol compound and / or carboxylic acid compound containing -OH is calculated based on the molar ratio of organic alcohol compound and / or carboxylic acid compound containing -OH to metal element of Group VIII; (5) according to the amount of Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound containing -OH, the modified alumina carrier is impregnated with the impregnation solution by pore saturation impregnation method, and then dried. Specifically, a phosphorus-containing compound is first dissolved in water to obtain a phosphorus-containing aqueous solution, and then an organic alcohol compound and / or a carboxylic acid compound containing -OH, a VIB group metal precursor and a VIII group metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is maintained to obtain an impregnation solution; (6) the water absorption rate of the modified alumina carrier is measured, and the liquid absorption rate of the modified alumina carrier is calculated according to the formula of water absorption rate of the modified alumina carrier-0.1; (7) according to the liquid absorption rate of the modified alumina carrier, the impregnation solution is adjusted to a corresponding volume (liquid absorption rate of the modified alumina carrier×mass of the carrier), and the impregnation solution and a corresponding mass of the modified alumina carrier are evenly mixed and allowed to stand, and then dried to prepare a hydrodenitrogenation catalyst.
[0072] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.
[0073] The third aspect of the present invention provides use of the hydrodenitrogenation catalyst described in the first aspect in a hydrodenitrogenation reaction.
[0074] In the present invention, the hydrodenitrogenation catalyst is used for the hydrodenitrogenation of distillate oil. Preferably, the nitrogen content in the distillate oil to be treated is 50-3000 ppm.
[0075] In a preferred embodiment, the catalyst needs to be converted from an oxidized catalyst to a sulfurized catalyst before use. In the present invention, there is no specific limitation on the sulfurization method, and conventional sulfurization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry sulfurization and wet sulfurization. There is no particular limitation on the type of the vulcanizing agent, and it can be selected according to conventional schemes in the art.
[0076] Preferably, the vulcanization conditions include: vulcanization temperature of 280-420°C, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1, and the preferred heating rate is 5-60°C / hour.
[0077] In a preferred embodiment, the conditions for hydrodenitrogenation include: pressure of 5-15 MPa, temperature of 260-410°C, volume space velocity of 0.5-10 hours -1 , the volume ratio of hydrogen to oil is 200-1000:1.
[0078] The catalyst provided by the invention has high hydrodenitrogenation performance when treating distillate oil, and the hydrodenitrogenation catalyst has good activity and stability.
[0079] The present invention will be described in detail below by way of examples. In the following examples, the hydrodenitrogenation performance of the catalyst was measured on a 20 mL high pressure microreactor. The catalyst was directly converted to a sulfurized state by a temperature programmed sulfurization method under the following conditions: the sulfurization pressure was 6.4 MPa, the sulfurized oil was kerosene containing 2 wt% CS2, and the volume space velocity was 2 hours. -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then increase the temperature to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodenitrogenation activity test, the reaction raw materials are high nitrogen distillate oil with a nitrogen content of 1154ppm. The test conditions are: pressure of 10MPa, volume space velocity of 1.5h -1 , the hydrogen-to-oil volume ratio was 800 v / v, and the reaction temperature was 340°C. After the reaction was stable for 2 days, the product properties were analyzed to obtain the nitrogen content in the product. The catalyst was deactivated at high temperature and high space velocity (temperature 390°C, volume space velocity 3.0 h -1 , time 3 days), at a pressure of 10 MPa and a volume space velocity of 1.5 hours -1 The test was carried out under the conditions of a hydrogen-to-oil volume ratio of 800 v / v and a reaction temperature of 340°C, and the nitrogen content in the product was analyzed to test the stability of the catalyst.
[0080] The composition of the catalyst is calculated based on the feed amount. The specific surface area of 2-100 nm, pore distribution, pore diameter, and pore volume in the catalyst and modified alumina carrier are determined by low-temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The mass fraction of nitrogen in the product is analyzed using a sulfur-nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0081] The feeding amount of each material in the following examples is determined according to the specific exemplary description given in the text of the present invention.
[0082] Example 1
[0083] A γ-alumina carrier was selected, and after the carrier was prepared, 2 wt% B2O3 was introduced by impregnation method to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 1.02 mL / g, and the specific surface area was 271 m 2 / g, the average pore size is 12.5nm, the pore volume with a pore size of 2-6nm accounts for 7.4% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0084] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0085] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0086] The atomic concentration of Mo in the catalyst is 6.7atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.29, P2O5 / MoO3 molar ratio is 0.13, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbonyl group is 0.485 nm, and the molar ratio of glycerol to Ni is 2.
[0087] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 161m 2 / g, pore volume 0.36cm 3 / g, the average pore size is 8.9nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 10.5% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 1.6ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 9.0ppm.
[0088] Example 2
[0089] Example 2 uses the same γ-alumina carrier as Example 1. After the carrier is prepared, 4 wt% P2O5 is introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier is 0.96 mL / g and the specific surface area is 269 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 7.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3.6% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0090] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0091] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0092] The atomic concentration of Mo in the catalyst is 12atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.785 nm, and the molar ratio of glycerol to Ni is 5.
[0093] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 149m 2 / g, pore volume 0.31cm 3 / g, the average pore size is 8.3nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 12.7% of the total pore volume. After the catalyst is sulfurized and reacted, the nitrogen content of the product is 0.8ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the product is 7.5ppm.
[0094] Example 3
[0095] The same γ-alumina carrier was used in Example 3 as in Example 1. After the carrier was prepared, 6 wt% SiO2 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.95 mL / g and the specific surface area was 275 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0096] MoO3, basic nickel carbonate and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a butterfly-shaped catalyst with a particle size of 1.6 mm.
[0097] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0098] The atomic concentration of Mo in the catalyst is 8.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.66 nm, and the molar ratio of glycerol to Ni is 3.
[0099] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 159m 2 / g, pore volume 0.33cm 3 / g, the average pore size is 8.3nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 11.5% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 1.1ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 8.3ppm.
[0100] Example 4
[0101] The same γ-alumina carrier was used in Example 4 as in Example 1. After the carrier was prepared, 2 wt% P2O5 was introduced by impregnation to obtain a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.97 mL / g and the specific surface area was 265 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 6.5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0102] Ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 5 hours, and dried at 130°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0103] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0104] The atomic concentration of W in the catalyst is 5.2atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.424 nm, and the molar ratio of citric acid to Ni is 2.
[0105] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 156m 2 / g, pore volume 0.37cm 3 / g, the average pore size is 9.5nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 8.5% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 1.0ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 8.0ppm.
[0106] Example 5
[0107] A γ-alumina carrier was selected, and 8 wt% SiO2 was introduced during the carrier preparation process to prepare a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.92 mL / g, and the specific surface area was 258 m 2 / g, the average pore size is 9.8nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0108] MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0109] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0110] The atomic concentration of Mo in the catalyst is 9.3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.12, (ai / ρ Xi +bi / ρ Yi+ci / ρ Zi ) / SA sup is 0.64 nm, and the molar ratio of citric acid to Ni is 2.
[0111] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 152m 2 / g, pore volume 0.36cm 3 / g, the average pore size is 9.5nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 10.2% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 1.2ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 8.6ppm.
[0112] Example 6
[0113] A γ-alumina carrier was selected, and 1.5 wt% B2O3 was introduced during the carrier preparation process to prepare a modified alumina carrier. The water absorption rate of the modified alumina carrier was 0.96 mL / g, and the specific surface area was 274 m 2 / g, the average pore size is 11.9nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 3% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm.
[0114] MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 160°C for 3 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0115] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0116] The atomic concentration of Mo in the catalyst is 9.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.27, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.83 nm, and the molar ratio of citric acid to Ni is 2.
[0117] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 133m 2 / g, pore volume 0.26cm3 / g, the average pore size is 7.8nm, the pore structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume with a pore size of 2-6nm accounts for 10.8% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 0.9ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 7.9ppm.
[0118] Example 7
[0119] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 4 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0120] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0121] The atomic concentration of Mo in the catalyst is 14atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.22, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 1.06nm, and the molar ratio of glycerol to Ni is 2.
[0122] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 124m 2 / g, pore volume 0.21cm 3 / g, the average pore size is 6.8nm, the structure shows a bimodal pore distribution characteristic at 2-6nm and 8-20nm, and the pore volume of 2-6nm accounts for 15.2% of the total pore volume. After sulfurization and reaction testing, the nitrogen content of the catalyst is 7.5ppm. After high-temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 32.5ppm.
[0123] Comparative Example 1
[0124] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0125] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0126] The atomic concentration of Mo in the catalyst is 3.8atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.28, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.322nm, and the molar ratio of glycerol to Ni is 2.
[0127] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 210m 2 / g, pore volume 0.46cm 3 / g, the average pore size is 8.8nm, the pore size distribution of the catalyst is a single peak pore, and the position of the single peak pore is 11.4nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content is 6.8ppm. After high temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 28.0ppm.
[0128] Comparative Example 2
[0129] The same modified alumina carrier as in Example 1 was selected to prepare a catalyst. MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0130] The modified alumina carrier and the amounts of the components are used so that the prepared catalyst satisfies:
[0131] The atomic concentration of Mo in the catalyst is 6.0atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.13, P2O5 / MoO3 molar ratio is 0.1, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SAsup The nanostructured carbon fiber is 0.38 nm, and the molar ratio of glycerol to Ni is 2.
[0132] After the catalyst was calcined at 400 degrees for 3 hours, its pore size distribution was analyzed by low-temperature nitrogen adsorption. The specific surface area of the catalyst is 186m 2 / g, pore volume 0.46cm 3 / g, the average pore size is 9.9nm, the pore structure shows a single peak pore distribution characteristic, and the single peak pore appears at 12.1nm. After the catalyst is sulfurized and tested for reaction, the nitrogen content is 5.2ppm. After high temperature catalytic deactivation, the denitrification activity is tested again, and the nitrogen content of the obtained product is 25.0ppm.
[0133] It can be seen from the data of the examples and comparative examples that the hydrodenitrogenation catalyst provided by the present invention has high activity and stability and good hydrodenitrogenation effect.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrodenitrogenation catalyst, in, The catalyst comprises a metal element of Group VIII, a metal element of Group VIB and a modified alumina carrier with a pore volume of 0.15-0.5 cm 3 / g, with an average pore size of 6-15nm, wherein the pore size of the catalyst presents a bimodal pore distribution in the range of 2-6nm and 8-20nm; The modified alumina carrier contains a weakly acidic component; The weakly acidic component is selected from at least one of B, P, Si, F and Ge elements; In the modified alumina carrier, the content of the weakly acidic component is 0.5-10% by weight, calculated as oxide; In the catalyst, the pore volume with a pore size distribution of 2-6 nm accounts for 7-15% of the total pore volume of the catalyst; The specific surface area of the catalyst is 110-200m 2 / g.
2. The catalyst according to claim 1, in, In the modified alumina carrier, B 2 O 3 The content is not more than 5% by weight, or P 2 O 5 The content is not more than 6% by weight, or SiO 2 The content is not more than 10% by weight, or the F content is not more than 5% by weight, or GeO 2 The content is not more than 6% by weight.
3. The catalyst according to claim 1 or 2, in, The water absorption rate of the modified alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 250 m 2 / g, the average pore size is greater than 9nm, and the pore distribution morphology is a unimodal pore distribution.
4. The catalyst according to claim 1 or 2, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the modified alumina carrier.
5. The catalyst according to claim 4, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 8% of the total pore volume of the modified alumina carrier.
6. The catalyst according to claim 1 or 2, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4% of the total pore volume of the modified alumina carrier.
7. The catalyst according to claim 6, in, In the modified alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 3% of the total pore volume of the modified alumina carrier.
8. The catalyst according to claim 1 or 2, in, In the catalyst, the pore volume with pore size distribution between 2-6 nm accounts for 8-13% of the total pore volume of the catalyst.
9. The catalyst according to claim 1 or 2, in, The average pore size of the catalyst is 6-12 nm.
10. The catalyst according to claim 1 or 2, in, The pore volume of the catalyst is 0.2-0.4 cm 3 / g.
11. The catalyst according to claim 1 or 2, in, Catalyst composition according to (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of the modified alumina support Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of the modified alumina support Yi, and Zi is P 2 O 5 , ci is relative to 1 gram of modified alumina support P 2 O 5 The mass of Sup refers to the modified alumina carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.4-1nm, ρ Xi , Yi , Zi are Group VIB metal oxides, Group VIII metal oxides and P 2 O 5 The density of SA sup is the specific surface area of the modified alumina support.
12. The catalyst according to claim 11, in, The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.4-0.85nm.
13. The catalyst according to claim 11, in, The molar ratio of Zi / Xi in the catalyst is 0.1-0.
4.
14. The catalyst according to claim 13, in, The molar ratio of Zi / Xi in the catalyst is 0.1-0.
35.
15. The catalyst according to claim 1 or 2, in, The atomic concentration of the VIB group metal elements in the catalyst on the surface of the modified alumina carrier is 4.5-14atom / nm 2 .
16. The catalyst according to claim 15, in, The atomic concentration of the VIB group metal elements in the catalyst on the surface of the modified alumina carrier is 5-12atom / nm 2 .
17. The catalyst according to claim 1 or 2, in, The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.1-0.
4.
18. The catalyst according to claim 16, in, The atomic ratio of the metal element of Group VIII to the total amount of the metal element of Group VIII and the metal element of Group VIB in the catalyst is 0.2-0.
3.
19. The catalyst according to claim 1 or 2, in, The catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds containing -OH, and the molar ratio of the organic alcohol compounds and / or carboxylic acid compounds to the metal element of Group VIII is 1-6.
20. The catalyst according to claim 19, in, The molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the Group VIII metal element is 2-5.
21. The catalyst according to claim 1 or 2, in, The equivalent diameter of the catalyst is 0.5-1.8 mm.
22. The catalyst according to claim 21, in, The equivalent diameter of the catalyst is 0.8-1.6 mm.
23. The catalyst according to claim 1 or 2, in, The catalyst is in the shape of a cylinder, a butterfly, a three-leaf clover, a four-leaf clover, a honeycomb or other irregular shapes.
24. A method for preparing a hydrodenitrogenation catalyst according to any one of claims 1 to 23, wherein the method include: The Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound and optionally the -OH-containing organic alcohol compound and / or the carboxylic acid compound are introduced into the modified alumina carrier by an impregnation method, and then dried.
25. The preparation method according to claim 24, in, The impregnation method comprises: impregnating the modified alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and optionally an organic alcohol compound containing -OH and / or a carboxylic acid compound.
26. The preparation method according to claim 25, in, The -OH-containing organic alcohol compound and / or carboxylic acid compound, Group VIII metal precursor, and Group VIB metal precursor are added to an aqueous solution of a phosphorus-containing compound to provide the impregnation solution.
27. The preparation method according to claim 24, in, The drying conditions include: temperature of 80-200° C. and time of 1-10 h.
28. Use of the hydrodenitrogenation catalyst according to any one of claims 1 to 23 in a hydrodenitrogenation reaction.