A purification process for lithium tetrafluoroborate

By using hydrolysis reaction and alkaline lithium salt to adjust pH value in the purification process of lithium tetrafluoroborate, the problem of high acidity and chloride ions in the purification of lithium tetrafluoroborate in the prior art was solved, and the high purity of tetrafluoroborate was achieved Lithium fluoroborate recycling meets the quality requirements of the lithium-ion battery industry and simplifies the process flow.

CN116040658BActive Publication Date: 2024-11-26HUBEI HUASHENG XIANGHE NEW ENERGY MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211696253.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-26
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

In the prior art, chloride ions are introduced into the purification process of lithium tetrafluoroborate, resulting in high acidity and chloride ions of the product lithium difluorooxalate borate, which is difficult to meet the quality requirements of the lithium-ion battery industry, and strong corrosion is generated during the reaction process. The hydrogen chloride gas affects the safety and environmental protection of the equipment.

Method used

The pure underwater hydrolysis reaction is used to add to the dried lithium tetrafluoroborate crude product, and alkaline lithium salt is added to adjust the pH value to form lithium tetrafluoroborate hydrate, and then dissolve by under reduced pressure, cooling, and non-aqueous polar solvent. Crystallization filter to remove insoluble matter, and obtain a high-purity lithium tetrafluoroborate product.

Benefits of technology

It realizes high-purity recycling of lithium tetrafluoroborate, reduces impurities, meets the quality requirements of the lithium-ion battery industry, simplifies the process flow, facilitates operation, and improves the recovery rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a purification process of lithium tetrafluoroborate, comprising: 1) adding pure water to the dried lithium tetrafluoroborate crude product, and performing a hydrolysis reaction at 60-90°C under stirring for 10-180 minutes; then slowly adding an alkaline lithium salt thereto, and adjusting the pH value to 5-8; 2) cooling and filtering, removing insoluble matter, obtaining a lithium tetrafluoroborate aqueous solution, and concentrating, crystallizing and filtering to obtain a lithium tetrafluoroborate hydrate; 3) drying the lithium tetrafluoroborate hydrate under reduced pressure at 70-140°C for 3-24 hours, cooling to room temperature under nitrogen, and then adding a non-aqueous polar solvent to stir and dissolve, filtering, and removing insoluble matter; 4) concentrating the filtrate under reduced pressure, adding a non-polar solvent for crystallization, washing and filtering, and vacuum drying to obtain an electronic grade lithium tetrafluoroborate product. The invention has the advantages of simple process, easy operation, and high purity and few impurities of the obtained lithium tetrafluoroborate after purification, which meets the requirements of the lithium ion battery industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium battery electrolyte preparation, and in particular relates to a purification process of lithium tetrafluoroborate. Background Art

[0002] Lithium oxalate and boron trifluoride complex are reacted to generate lithium difluorooxalate borate and lithium tetrafluoroborate, and then the lithium difluorooxalate borate product is obtained after repeated recrystallization, purification and separation. As a by-product, lithium tetrafluoroborate contains a large amount of lithium difluorooxalate borate that has not been completely separated, resulting in low purity and more impurities such as acidity, which makes it difficult to meet the quality requirements of the lithium-ion battery industry. In order to achieve the recycling of lithium tetrafluoroborate, a by-product of the above process, the method currently used is: in a non-aqueous organic solvent, under the action of the auxiliary reaction reagent silicon tetrachloride, lithium tetrafluoroborate reacts with anhydrous oxalic acid to generate lithium difluorooxalate borate. The main problem of this method is that chloride ions are introduced during the reaction, resulting in high acidity and chloride ions in the product lithium difluorooxalate borate, which is difficult to meet the quality requirements of the lithium-ion battery industry; at the same time, highly corrosive hydrogen chloride gas is generated during the reaction, which has high requirements for equipment, safety and environmental protection. Summary of the invention

[0003] 1. Technical problems to be solved

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a purification process for lithium tetrafluoroborate, wherein lithium oxalate and a boron trifluoride complex are reacted to generate lithium difluorooxalate borate and lithium tetrafluoroborate, and then the byproduct lithium tetrafluoroborate is obtained after repeated recrystallization, purification and separation to obtain the lithium difluorooxalate borate product, and then the byproduct lithium tetrafluoroborate is recovered and purified. The process is simple and easy to operate. After purification, the obtained lithium tetrafluoroborate has high purity and few impurities, which meets the requirements of the lithium ion battery industry.

[0005] 2. Technical solution

[0006] In order to achieve the above purpose and the above technical effect, the present invention adopts the following technical solution:

[0007] A purification process for lithium tetrafluoroborate, characterized in that it comprises the following steps:

[0008] 1) adding pure water to the dried crude lithium tetrafluoroborate, and performing a hydrolysis reaction at 60-90° C. with stirring for 10-180 min; then slowly adding an alkaline lithium salt thereto, and adjusting the pH value to 5-8; the crude lithium tetrafluoroborate is a mixture of lithium tetrafluoroborate and lithium difluorooxalatoborate;

[0009] 2) cooling and filtering to remove insoluble matter to obtain a lithium tetrafluoroborate aqueous solution, and concentrating, crystallizing and filtering to obtain lithium tetrafluoroborate hydrate;

[0010] 3) drying lithium tetrafluoroborate hydrate at 70-140° C. under reduced pressure for 3-24 hours, cooling to room temperature under nitrogen, adding a non-aqueous polar solvent, stirring to dissolve, filtering, and removing insoluble matter;

[0011] 4) The filtrate is concentrated under reduced pressure, a non-polar solvent is added for crystallization, the mixture is washed, filtered, and vacuum dried to obtain an electronic grade lithium tetrafluoroborate product.

[0012] Furthermore, the preparation process of the crude lithium tetrafluoroborate is as follows: a boron trifluoride complex and lithium oxalate are reacted, and then purified by recrystallization to obtain a by-product crude lithium tetrafluoroborate, which has a lithium tetrafluoroborate content of 70% to 95% and a lithium difluorooxalatoborate content of 30% to 5%.

[0013] Furthermore, the crude lithium tetrafluoroborate is dried at a temperature of 40° C. to 80° C. and a pressure of 5 to 30 KPa.

[0014] Furthermore, the amount of pure water added is 2 to 6 times the quality of crude lithium tetrafluoroborate.

[0015] Furthermore, the alkaline lithium salt is selected from lithium hydroxide, lithium carbonate or a mixture thereof.

[0016] Furthermore, the non-aqueous polar solvent is selected from one or a mixture of two or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, acetonitrile, propionitrile, methyl acetate, ethyl acetate, propyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, acetone, methyl ethyl ketone, 1,4-dioxane, 1,4-butyrolactone, tetrahydrofuran, and ethylene glycol dimethyl ether.

[0017] Furthermore, the amount of the non-aqueous polar solvent added is 2 to 5 times the quality of the crude lithium tetrafluoroborate after drying, and the dissolution time is 10 to 180 minutes.

[0018] Furthermore, the non-polar solvent is selected from one or a mixture of two or more of benzene, toluene, p-xylene, m-xylene, o-xylene, chlorobenzene, n-hexane, cyclohexane, n-heptane, n-octane, dichloromethane, 1,2-dichloroethane, trichloroethane, tetrachloroethane, and petroleum ether.

[0019] The purification principle of the present invention is that a small amount of unseparated lithium difluorooxalatoborate in the crude lithium tetrafluoroborate undergoes a hydrolysis reaction under the action of pure water to generate lithium tetrafluoroborate hydrate LiBF4·H2O and lithium bis(oxalatoborate) LiB(C 2 O 4 ) 2 , the reaction formula is as follows:

[0020] 2LiF 2 BC 2 O 4 +H 2O→LiBF4·H 2 O+LiB(C 2 O 4 ) 2

[0021] The generated lithium bis(oxalatoborate) LiB(C 2 O 4 ) 2 The hydrolysis reaction continues to generate boric acid, oxalic acid and lithium hydrogen oxalate. The reaction formula is as follows:

[0022] LiB(C 2 O 4 ) 2 +3H 2 O→LiOOCCOOH+H 3 BO 3 +H 2 C 2 O 4

[0023] The hydrolysis products, lithium hydrogen oxalate, oxalic acid and boric acid, continue to react with alkaline lithium salts to generate lithium oxalate and lithium borate that are insoluble or slightly soluble in water. They can be removed by cooling and filtering. The lithium tetrafluoroborate hydrate obtained above is dried under reduced pressure at 70-140°C for 3-24 hours, cooled to room temperature under nitrogen, and then non-aqueous polar solvent is added to stir and dissolve, filtered, and insoluble matter is removed. The filtrate is concentrated under reduced pressure, a non-polar solvent is added to crystallize, washed, filtered, and vacuum dried to obtain an electronic grade lithium tetrafluoroborate product.

[0024] 3. Beneficial effects

[0025] Compared with the prior art, the invention has the following beneficial effects: the process is simple and easy to operate, and the byproduct lithium tetrafluoroborate obtained by synthesizing lithium difluorooxalatoborate can be effectively recovered with a high recovery rate; after purification, the obtained lithium tetrafluoroborate has high purity and few impurities, meeting the requirements of the lithium ion battery industry. DETAILED DESCRIPTION

[0026] The present invention will be described in further detail below in conjunction with specific embodiments to make the advantages of the present invention more obvious. It should be understood that the contents thereof are only for illustration and are not intended to limit the scope of protection of the present invention. The experimental methods in the following embodiments that do not specify specific conditions are usually carried out under normal conditions or under conditions recommended by the manufacturer. Unless otherwise stated, all parts are by weight and all percentages are by weight.

[0027] Example 1

[0028] The crude lithium tetrafluoroborate byproduct of the synthesis of lithium difluorooxalatoborate was taken and dried at 40°C and 5KPa under negative pressure for 5 hours to remove the organic solvent dimethyl carbonate. After testing, the lithium tetrafluoroborate content was measured by ion chromatography to be 70.6%, and the acidity test method was γ-butyrolactone titration with anhydrous triethylamine, the indicator was neutral red-methylene blue, and the acidity was measured to be 1250ppm.

[0029] 200 g of the dried crude lithium tetrafluoroborate was added into a three-necked flask with stirring, and then 400 g of pure water was added thereto. The temperature was raised to 90°C with stirring and the reaction was carried out for 10 minutes. Then, lithium hydroxide was slowly added thereto in batches until the pH value reached 5.

[0030] After completion, the temperature was lowered to 30-35°C and filtered to obtain a transparent clear liquid. The temperature was raised under reduced pressure and concentrated until the residual volume was about 60%, and evaporation was stopped. The temperature was lowered to 20-25°C for crystallization for 5 hours, and filtered. The filter cake was white lithium tetrafluoroborate hydrate. The filter cake was dried under reduced pressure at 70-75°C and 5KPa for 24 hours, and cooled in a nitrogen atmosphere to obtain 136g of dried lithium tetrafluoroborate.

[0031] The above lithium tetrafluoroborate was added to 270g of acetonitrile with a water content of 108ppm, stirred and dissolved for 30min at room temperature and normal pressure, filtered with a 0.45μm PTFE filter membrane, and the filtrate was concentrated under reduced pressure until solids were precipitated, and then 200g of dichloromethane was added to stir and crystallize, filtered, and then rinsed twice with 100g of dichloromethane, and vacuum dried to obtain 128g of lithium tetrafluoroborate product with a recovery rate of 91%. After testing, the purity was 99.96%, the water content was 48ppm, and the acidity (in terms of HF) was 16ppm.

[0032] Example 2

[0033] The crude lithium tetrafluoroborate byproduct of the synthesis of lithium difluorooxalatoborate was dried at 80°C and 30KPa under negative pressure for 1 hour to remove the organic solvent. After testing, the lithium tetrafluoroborate content was measured by ion chromatography to be 94.8%, and the acidity test method was γ-butyrolactone titration with anhydrous triethylamine, the indicator was neutral red-methylene blue, and the acidity was measured to be 869ppm.

[0034] 100 g of the dried crude lithium tetrafluoroborate was added into a three-necked flask with stirring, and then 600 g of pure water was added thereto. The temperature was raised to 60°C with stirring and the reaction was carried out for 30 minutes. Then, lithium carbonate was slowly added thereto in batches until the pH value reached 8.

[0035] After completion, cool to room temperature and filter to obtain a transparent clear liquid. Heat and concentrate under reduced pressure until the content of lithium tetrafluoroborate is about 70%, stop evaporation, cool to 10-15°C for crystallization for 2 hours, filter, and the filter cake is white lithium tetrafluoroborate hydrate. Dry the filter cake under reduced pressure at 130-140°C and 5-10KPa for 3 hours, cool in a nitrogen atmosphere, and obtain 87g of dried lithium tetrafluoroborate.

[0036] The lithium tetrafluoroborate was added to 430g of ethanol with a water content of 126ppm, stirred and dissolved at room temperature and normal pressure for 10min, filtered with a 0.1μm PTFE filter membrane, and the filtrate was concentrated under reduced pressure until solids were precipitated. Then, 100g of toluene was added to stir and crystallize, filtered, and rinsed once with 60g of toluene. After vacuum drying, 83g of lithium tetrafluoroborate product was obtained, and the recovery rate was 88%. After testing, the purity was 99.94%, the water content was 65ppm, and the acidity (in terms of HF) was 6ppm.

[0037] Example 3

[0038] The crude lithium tetrafluoroborate byproduct of the synthesis of lithium difluorooxalatoborate was dried at 65-70°C and 10-15KPa under negative pressure for 3 hours to remove the organic solvent. After testing, the lithium tetrafluoroborate content was measured by ion chromatography to be 87.5%, and the acidity was measured to be 1860ppm by γ-butyrolactone titration with anhydrous triethylamine and neutral red-methylene blue as the indicator.

[0039] 180 g of the dried crude lithium tetrafluoroborate was added into a three-necked flask with stirring, and then 540 g of pure water was added thereto. The temperature was raised to 70-75°C with stirring and the reaction was carried out for 180 minutes. Then, lithium hydroxide was slowly added thereto in batches until the pH value reached 6-7.

[0040] After completion, the mixture was cooled to room temperature and filtered to obtain a transparent clear liquid. The mixture was concentrated under reduced pressure until the content of lithium tetrafluoroborate was about 65-75%, and then the evaporation was stopped. The mixture was cooled to 15-18°C for crystallization for 3 hours and filtered. The filter cake was a white lithium tetrafluoroborate hydrate. The filter cake was dried at 100-110°C under reduced pressure of 15-20KPa for 6 hours and cooled in a nitrogen atmosphere to obtain 142g of dried lithium tetrafluoroborate.

[0041] The lithium tetrafluoroborate was added to 425g of dimethyl carbonate with a water content of 59ppm, stirred and dissolved at room temperature and normal pressure for 60min, filtered with a 0.1μm PTFE filter membrane, and the filtrate was concentrated under reduced pressure until solids were precipitated, and then 180g of petroleum ether was added to stir and crystallize, filtered, and rinsed once with 100g of petroleum ether, and vacuum dried to obtain 136g of lithium tetrafluoroborate product with a recovery rate of 86%. After testing, the purity was 99.98%, the water content was 35ppm, and the acidity (in terms of HF) was 11ppm.

[0042] It should be understood that after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A purification process for lithium tetrafluoroborate, characterized in that: The following steps are involved: 1) adding pure water to the dried crude lithium tetrafluoroborate, and performing a hydrolysis reaction at 60-90° C. with stirring for 10-180 min; then slowly adding lithium hydroxide or lithium carbonate to the crude lithium tetrafluoroborate, and adjusting the pH value to 5-8; the crude lithium tetrafluoroborate is a mixture of lithium tetrafluoroborate and lithium difluorooxalatoborate; 2) Cooling and filtering to remove insoluble matter to obtain a lithium tetrafluoroborate aqueous solution, which is then concentrated, crystallized and filtered to obtain lithium tetrafluoroborate hydrate; 3) Dry lithium tetrafluoroborate hydrate at 70-140°C under reduced pressure for 3-24 hours, cool to room temperature under nitrogen, add a non-aqueous polar solvent, stir to dissolve, filter, and remove insoluble matter; 4) The filtrate is concentrated under reduced pressure, a non-polar solvent is added for crystallization, the product is washed, filtered, and vacuum dried to obtain an electronic grade lithium tetrafluoroborate product.

2. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The preparation process of the crude lithium tetrafluoroborate is as follows: a boron trifluoride complex and lithium oxalate are reacted, and then purified by recrystallization to obtain a byproduct crude lithium tetrafluoroborate, wherein the content of the lithium tetrafluoroborate is 70% to 95% and the content of the lithium difluorooxalatoborate is 30% to 5%.

3. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The drying temperature of the crude lithium tetrafluoroborate is 40° C. to 80° C., and the pressure is 5 to 30 KPa.

4. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The amount of pure water added is 2 to 6 times the mass of crude lithium tetrafluoroborate.

5. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The non-aqueous polar solvent is selected from one or a mixture of two or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, acetonitrile, propionitrile, methyl acetate, ethyl acetate, propyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, acetone, methyl ethyl ketone, 1,4-dioxane, 1,4-butyrolactone, tetrahydrofuran, and ethylene glycol dimethyl ether.

6. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The amount of the non-aqueous polar solvent added is 2 to 5 times the mass of the crude lithium tetrafluoroborate after drying, and the dissolution time is 10 to 180 minutes.

7. A purification process for lithium tetrafluoroborate according to claim 1, characterized in that: The non-polar solvent is selected from one or a mixture of two or more of benzene, toluene, p-xylene, m-xylene, o-xylene, chlorobenzene, n-hexane, cyclohexane, n-heptane, n-octane, dichloromethane, 1,2-dichloroethane, trichloroethane, tetrachloroethane and petroleum ether.

Citation Information

Patent Citations

  • A synthetic method of electronic grade lithium difluoro(oxalato)borate

    CN105859760A

  • Preparation method for lithium tetrafluoroborate

    CN106082251A

  • Preparation method of lithium oxalyldifluoroborate

    CN111171061A

  • Purification method of lithium tetrafluoroborate

    CN111204776A

  • Method for preparing high-purity lithium salt by mixing in a predetermined ratio and its application

    JP6740424B1