Coal gangue solid waste-based paste filling pipeline flushing-free material and filling process
Through the combination of A slurry and B slurry of coal gangue solid waste base paste filling material, the problems of complex and low efficiency of traditional filling processes are solved, efficient and low-cost mine filling is achieved, process flow is simplified, and solid waste utilization is improved reduces environmental pollution.
Patent Information
- Application Number
- CN202211739416.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The traditional coal gangue filling process is complex and the filling efficiency is low. It requires multiple flushing and processes, resulting in high production costs, waste of resources and environmental pollution.
The coal gangue solid waste base paste filling material is used, and through the combination of A slurry and B slurry, A slurry maintains fluidity in the pipeline. After the addition of B slurry, it quickly condenses to form an overall strength, simplifies the process flow and reduces the flushing steps.
It improves the performance of filling materials, reduces engineering costs, simplifies process flow, increases solid waste utilization, realizes efficient mine filling, reduces environmental pollution, and has broad market promotion prospects.
Smart Images

Figure CN116041013B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mine filling materials, and in particular to a gangue solid waste-based paste-filled pipeline flushing-free material and a filling process. Background Art
[0002] In the coal industry, a large amount of coal gangue is discharged during coal production and coal washing, and is usually treated as solid waste. However, my country has entered the peak period of mineral resource consumption, and the coal mining industry faces geological disasters such as deep rock bursts and rock bursts, ecological and environmental problems such as surface subsidence and collapse, and technical and economic problems such as production capacity and production costs. Due to the deterioration of the natural ecological environment caused by the discharge of a large amount of industrial wastewater, waste, and waste gas, the environmental and ecological problems caused by coal mining are becoming increasingly prominent.
[0003] Backfill mining can improve coal recovery rate, make full use of resources, effectively control ground pressure and reduce surface subsidence. The preparation of backfill materials is a key link in backfill mining. Backfilling of goafs is mainly to fill the remaining voids and mining cracks in the goafs, and the consumption of backfill materials is often huge.
[0004] In the traditional filling process, it is necessary to carry out air blowing and water pumping in sequence to clear and clean the pipes, followed by filling mortar and gangue slurry. After the material filling is completed, the pipes need to be cleaned again by pumping water. The filling process is relatively complicated and the filling efficiency is low. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention provides a coal gangue solid waste-based paste-filled pipeline flushing-free material and a filling process.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] On the one hand, the present invention provides a coal gangue solid waste-based paste-filled pipeline flushing-free material, characterized in that it includes a slurry A and a slurry B used in combination, wherein:
[0008] Slurry A includes the following components and their weight proportions: 98-99 parts of coal gangue powder, 0.5-2 parts of retarder, and 0.03-0.05 parts of hydroxypropyl methylcellulose ether;
[0009] The B slurry includes the following components and their mass proportions: 10-25 parts of cement clinker, 20-30 parts of fly ash, 30-45 parts of coal gangue, 0.3-1 parts of concrete latex powder, and 1.5-2.5 parts of accelerator.
[0010] The preparation of slurry A is as follows: each component in slurry A is mixed with water in proportion.
[0011] The preparation of B slurry is as follows: mix cement clinker, fly ash, coal gangue, concrete latex powder and accelerator.
[0012] Furthermore, the retarder includes rock honey and a water reducing agent.
[0013] Furthermore, the weight ratio of rock honey to water reducing agent ranges from 9:1 to 8:2.
[0014] Furthermore, the rock honey has an aldehyde group and a hydroxyl group.
[0015] Furthermore, the water reducing agent is a polycarboxylic acid water reducing agent.
[0016] Furthermore, the preparation method of the accelerating setting agent is: preparing the accelerating setting agent by physically mixing and modifying multiple components such as alumina clinker, soda ash, thickener, etc.
[0017] On the other hand, the present invention provides a filling process, characterized in that the above-mentioned slurry A is first filled into the filling pipeline to maintain its fluidity in the pipeline, and then the above-mentioned slurry B is filled into the end of the filling pipeline, so that the slurry A and the slurry B are evenly mixed at the discharge port of the filling pipeline by a mixing and stirring device, and the slurry produces overall strength after mixing.
[0018] Among them, slurry A can maintain good flow properties within 24h-48h of filling the pipeline, and after merging with slurry B, the material can solidify in a short time to generate strength.
[0019] The beneficial effects of the present invention are:
[0020] 1. The present invention utilizes solid waste resources such as coal gangue as a paste filling and flushing-free material, which can not only reduce engineering costs, effectively improve the performance of filling materials, simplify the filling process, but also increase the comprehensive utilization rate of solid waste, which is of great significance to the development of mine filling and mining industry;
[0021] 2. The present invention uses the independent A slurry and B slurry in combination, and the A slurry can be filled in the pipeline, which has good flow performance in the short term. When filling the material, a certain amount of B slurry must be filled first, and then the gangue slurry can be directly filled, saving the process of blasting, water pumping, and mortar. When the A slurry and the B slurry are mixed, the mixed material can produce overall strength to meet the safety performance requirements of the engineering project.
[0022] 3. A slurry still maintains good flowability within 24h-48h of filling the pipeline. When B slurry is added, the mixed material can coagulate and generate strength in a short time, wherein the coagulation time is controlled at about 5h, and the material's compressive strength is about 1.6MPa in 3 days. The preparation process of pipeline flushing-free material is simple and the production cost is low, so the patent of this invention has a broad market promotion prospect, and is also of great significance to the reuse of waste resources and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a schematic diagram of slurry A of Example 1;
[0024] Figure 2 This is a diagram of the material after filling with slurry B in Example 1. DETAILED DESCRIPTION
[0025] The principles and features of the present invention are described below. The examples given are only used to explain the present invention but not to limit the scope of the present invention.
[0026] Example 1
[0027] The paste filling material of this embodiment includes:
[0028] A slurry: comprising the following components by weight: 98 parts of coal gangue powder, 0.9 parts of rock honey, 0.1 parts of water reducing agent, and 0.03 parts of hydroxypropyl methylcellulose ether;
[0029] B slurry: includes the following components by mass: 15 parts of cement clinker, 30 parts of fly ash, 30 parts of coal gangue, 2 parts of concrete latex powder, and 1.5 parts of accelerator.
[0030] Slurry A and slurry B are used together in the filling process. The specific preparation method is as follows:
[0031] Add 98 parts of coal gangue powder, 0.9 parts of rock honey, 0.1 parts of water reducer, and 0.03 parts of hydroxypropyl methylcellulose ether to an appropriate amount of stirring water, stir slowly for 120 seconds, and stir quickly for 60 seconds to obtain slurry A. Mix 15 parts of cement clinker, 30 parts of fly ash, 30 parts of coal gangue, 2 parts of concrete latex powder, and 1.5 parts of accelerator and stir evenly, then add a certain amount of water and stir for 3 minutes to obtain slurry B. When filling the material, first fill the A slurry into the pipeline, and mix the B slurry with the A slurry through a mixing device at the outlet of the filling pipeline, and finally form a flush-free material for filling the pipeline.
[0032] Example 2
[0033] The paste filling material of this embodiment includes:
[0034] A slurry: comprising the following components by weight: 98 parts of coal gangue powder, 1.6 parts of rock honey, 0.4 parts of water reducing agent, and 0.05 parts of hydroxypropyl methylcellulose ether;
[0035] B slurry: includes the following components in parts by mass: 20 parts of cement clinker, 25 parts of fly ash, 45 parts of coal gangue, 1 part of concrete latex powder, and 2.5 parts of accelerator.
[0036] Slurry A and slurry B are used together in the filling process. The specific preparation method is as follows:
[0037] Add 98 parts of coal gangue powder, 1.6 parts of rock honey, 0.4 parts of water reducer, and 0.05 parts of hydroxypropyl methylcellulose ether to an appropriate amount of stirring water, stir slowly for 120 seconds, and stir quickly for 60 seconds to obtain slurry A. Mix 20 parts of cement clinker, 25 parts of fly ash, 45 parts of coal gangue, 1 part of concrete latex powder, and 2.5 parts of accelerator and stir evenly, then add a certain amount of water and stir for 3 minutes to obtain slurry B. When filling the material, first fill the A slurry into the pipeline, and mix the B slurry with the A slurry through a mixing device at the outlet of the filling pipeline to form a flush-free material for filling the pipeline.
[0038] Example 3
[0039] The paste filling material of this embodiment includes:
[0040] A slurry: comprising the following components by weight: 99 parts of coal gangue powder, 0.45 parts of rock honey, 0.05 parts of water reducing agent, and 0.04 parts of hydroxypropyl methylcellulose ether;
[0041] B slurry: includes the following components in parts by mass: 10 parts of cement clinker, 25 parts of fly ash, 35 parts of coal gangue, 0.8 parts of concrete latex powder, and 2 parts of accelerator.
[0042] Slurry A and slurry B are used together in the filling process. The specific preparation method is as follows:
[0043] Add 99 parts of coal gangue powder, 0.45 parts of rock honey, 0.05 parts of water reducer, and 0.04 parts of hydroxypropyl methylcellulose ether to an appropriate amount of stirring water, stir slowly for 120 seconds, and stir quickly for 60 seconds to obtain slurry A. Mix 10 parts of cement clinker, 25 parts of fly ash, 35 parts of coal gangue, 0.8 parts of concrete latex powder, and 2 parts of accelerator and stir evenly, then add a certain amount of water and stir for 3 minutes to obtain slurry B. When filling the material, first fill the A slurry into the pipeline, and mix the B slurry with the A slurry through a mixing device at the outlet of the filling pipeline to complete the preparation of the flush-free material for filling the pipeline.
[0044] In the above embodiment, the cement clinker is 32.5R fly ash silicate cement; the coal gangue is produced by Daizhuang Coal Mine in Jining area, and the SiO2 content reaches more than 50%, and the Al2O3 content is more than 15%; the coal gangue powder is ground by a VB-2 / 100 sealed ball mill for 2 minutes, and the discharge particle size is about 80-200 mesh; the concrete latex powder is a water-soluble redispersible powder with a bulk density of 300-500g / L and a solid content of ≥98.0wt%; the fly ash is Class II fly ash, and the 45μm square hole sieve residue is not more than 25%; the accelerator is mainly prepared by modifying multiple components such as alumina clinker, soda ash, thickener, etc., with a fineness of less than 12.6%, an initial setting time of 2-3min, and a final setting time of 8-10min; the hydroxypropyl methylcellulose ether model is WTM0008 400pf.
[0045] The specific filling process of the paste filling material of the above-mentioned embodiment is as follows: when filling the underground minerals, firstly, air blowing and water pumping are carried out in sequence to clear and clean the pipeline, and then the filling process of the slurry material is carried out. When the underground filling cycle is about to end, the above-mentioned A slurry is pumped into the filling pipeline, one is to remove the residual materials in the pipeline, and the other is to keep the A slurry in the pipeline until the next filling cycle. At the beginning of the next cycle of filling, a mixing and stirring device is used at the discharge port of the filling pipeline to achieve uniform mixing of the A slurry and the B slurry, so as to promote the strength of the mixed slurry in a short time. At the same time, the slurry material filling process can be carried out directly without the need to carry out the pipeline cleaning processes such as air blowing and water pumping again, that is, the air blowing and water pumping processes after filling in the previous cycle and the air blowing and water pumping processes before filling in the next cycle are saved, which greatly simplifies the filling process and improves the underground filling efficiency.
[0046] In addition, a separate structural design can be performed on the material filling pipeline discharge port. A spiral self-stirring device is built into the discharge port pipeline. During the flow of the filling material, the self-stirring device will automatically rotate with the flow of the material, which ensures that after the B liquid is added to the A liquid, it can be evenly stirred for full reaction, and at the same time effectively avoids the filling material blocking the pipe due to the self-stirring device.
[0047] The performance tests of the filling pipe flushing-free materials prepared in the above embodiments 1-3 were carried out. The fluidity was in accordance with the "Method for Determination of Fluidity of Cement Mortar" (GB / T2419-2005); the setting time was in accordance with the "Test Method for Water Consumption, Setting Time and Stability of Cement Standard Consistency" (GB / T1346-2011); the compressive strength of the material was tested in accordance with the "Standard Test Method for Basic Properties of Building Mortar" (JGJ / T70-2009). The test results are shown in Table 1.
[0048] Table 1 Performance test results of filling pipeline flush-free materials
[0049]
[0050] The above is only an embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A filling process, It is characterized in that First, fill the filling pipeline with slurry A to maintain its fluidity in the pipeline, and then fill the end of the filling pipeline with slurry B, so that slurry A and slurry B are evenly mixed at the discharge port of the filling pipeline using a mixing and stirring device, and the slurry produces overall strength after mixing; Slurry A includes the following components and their weight proportions: 98-99 parts of coal gangue powder, 0.5-2 parts of retarder, and 0.03-0.05 parts of hydroxypropyl methylcellulose ether; The B slurry includes the following components and their mass proportions: 10-25 parts of cement clinker, 20-30 parts of fly ash, 30-45 parts of coal gangue, 0.3-1 parts of concrete latex powder, and 1.5-2.5 parts of accelerator.
2. The filling process according to claim 1, It is characterized in that The retarder comprises rock honey and a water reducing agent.
3. The filling process according to claim 2, It is characterized in that The weight ratio of rock honey to water reducing agent ranges from 9:1 to 8:
2.
4. The filling process according to claim 2, It is characterized in that The rock honey has an aldehyde group and a hydroxyl group.
5. The filling process according to claim 2, It is characterized in that The water reducing agent is a polycarboxylic acid water reducing agent.
Citation Information
Patent Citations
Pumped pasty fluid mining with filling pipeline cleaning-free process technology
CN110617104A
Cemented filling material for coal mines and preparation method thereof
CN111018443A