Method for preparing 2-propyl-1-heptanol

By using alumina microsphere support to support metal active components in the enalde hydrogenation reaction, the problems of high cost of noble metal catalysts and metal chromium pollution are solved, and 2-propyl-1-heptol are improved Selectivity and conversion rate achieve simplification of the process and reduction of energy consumption.

CN116041142BActive Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111264935.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-11-22
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

The use of precious metal catalysts in the existing enaldehyde hydrogenation and alkanol production technology leads to high costs, and the use of metal chromium leads to environmental pollution. The multi-step hydrogenation process is complex and is not suitable for industrial applications.

Method used

The carrier is prepared by contacting alumina microspheres with nitrogen-containing polymer solution and then calcining it, and then loading the metal active components. The 2-propyl-2-heptenal hydrogenation reaction is carried out through one-step hydrogenation method to prepare 2-propyl- 1-Heptyl alcohol, avoid the use of precious metals and metal chromium.

Benefits of technology

Improve the conversion rate of 2-propyl-2-heptenal and selectivity of 2-propyl-1-heptol, reduce the generation of by-products, reduce the energy consumption of subsequent distillation separation, and achieve the purpose of energy saving and emission reduction .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003326515900000081
    Figure BDA0003326515900000081
  • Figure BDA0003326515900000101
    Figure BDA0003326515900000101
  • Figure BDA0003326515900000111
    Figure BDA0003326515900000111
Patent Text Reader

Abstract

The present invention relates to the technical field of alkanol hydrogenation, and discloses a method for preparing 2-propyl-1-heptanol, the method comprising: in the presence of a catalyst, 2-propyl-2-heptenal is contacted with hydrogen to produce a hydrogenation reaction; wherein, the preparation method of the catalyst comprises: contacting alumina microspheres with a nitrogen-containing polymer solution, and then first calcining the contact product under an inert atmosphere to obtain a carrier, and then loading the metal active component on the carrier. The method of the present invention can improve the selectivity of 2-propyl-1-heptanol under the premise of ensuring the conversion rate of 2-propyl-2-heptenal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparing alkanols by hydrogenating enal, and in particular to a method for preparing 2-propyl-1-heptanol. Background Art

[0002] In recent years, due to the safety and environmental protection of plasticized products, the industry has begun to use alcohols with higher carbon numbers to produce plasticizers, and decanol is one of them. 2-propyl-1-heptanol is one of the important representatives of decanol. The existing routes for producing 2-propyl-1-heptanol mainly include: (1) obtaining C9 olefins through trimerization of propylene or oligomerization of propylene and butene, and then undergoing carbonyl synthesis and hydrogenation to produce 2-propyl-1-heptanol; (2) butene is hydroformylated to synthesize valeraldehyde, which is then condensed to produce 2-propyl-2-heptenal, and then hydrogenated to obtain 2-propyl-1-heptanol.

[0003] CN101185893A discloses a catalyst for gas phase hydrogenation of decenal to produce isodecanol and a preparation method thereof. The catalyst is prepared by coprecipitation method and is composed of copper oxide, zinc oxide, aluminum oxide and an active agent; the active agent is one or more metal element compounds of Na, K, Ni, Co, Mg, Ca, and Ba; the molar contents of copper oxide, zinc oxide, and aluminum oxide are 20-70%, 28-70%, and 1-10%, respectively, and the active agent is present in a molar content of 0.1-2.0%. The catalyst is used for gas phase hydrogenation of decenal to produce isodecanol and has a high decenal conversion rate and isodecanol selectivity. However, the gas phase hydrogenation reaction needs to be carried out at 140-180°C, and subsequent condensation separation is required, which has high energy consumption and complex process.

[0004] CN1883795A discloses a method for preparing a copper-zinc-aluminum gas-phase aldehyde hydrogenation catalyst, wherein the active components are 10-60% CuO, 20-80% ZnO, and 0.1-20% Al2O3, and graphite is used as a carrier to form a tablet to obtain the catalyst. The step-by-step continuous coprecipitation method is adopted to change the step-by-step intermittent feeding method into a continuous feeding method, and the obtained catalyst has a large specific surface area and pore volume, a high dispersion of active metal copper, and a greatly improved catalyst activity. However, the gas phase reaction method requires the raw material aldehyde to be gasified, and for decenaldehyde, it is easy to polymerize during the gasification phase change process, which reduces the selectivity of the target product alcohol.

[0005] CN102666455A A method for preparing decanol by hydrogenating decanal. The method requires at least two reactors, wherein the first reactor uses a copper-based and / or nickel-based catalyst, and the second reactor uses a palladium or ruthenium catalyst, both of which are carried out in a liquid phase on a solid catalyst. The method can hydrogenate decanal into decanol in high yield, and the content of unsaturated decanal in the hydrogenation discharge is less than 1500ppm. The hydrogenation method of the invention is relatively complicated, using multiple reactors in series, and the second reactor uses an expensive noble metal catalyst.

[0006] CN104513131B discloses a method for preparing decanol by liquid phase hydrogenation of decanal. The method uses a Raney nickel catalyst supported by an organic polymer, and decanal flows through a catalyst bed in a liquid state under a hydrogen atmosphere, and decanol can be obtained with high yield and high selectivity. However, the catalyst is Raney nickel, which is relatively expensive and has a certain combustion risk during use.

[0007] CN106179373A proposes a catalyst for preparing isodecyl alcohol by liquid phase hydrogenation of decanal and a preparation method thereof. The three active components of nickel, copper and chromium are loaded onto an alumina carrier by a precipitation method, and the obtained catalyst has a high isodecyl aldehyde conversion rate and isodecyl alcohol selectivity. However, the presence of chromium will cause great harm to the environment and health.

[0008] CN113019378A discloses an olefinic aldehyde hydrogenation catalyst, which can be used for preparing decanol by hydrogenation of decene aldehyde, and comprises: NiO 5-50%, CuO 5-25%, MgO 0.1-10%, and the balance is γ-Al2O3. The catalyst is prepared by mixing γ-alumina powder, a magnesium source and a water-soluble organic matter, and then undergoing solid-liquid separation, sequentially undergoing first drying and first calcination to obtain a product as an intermediate carrier; the obtained intermediate carrier, an alumina precursor and an additive are mixed, and then sequentially undergoing molding, second drying and second calcination to obtain a carrier; the carrier is impregnated with a mixed solution containing nickel and copper, and sequentially undergoing third drying and third calcination after solid-liquid separation to obtain the olefinic aldehyde hydrogenation catalyst. It has good anti-coking performance and catalytic activity, and can extend the service life of the catalyst. However, the catalyst belongs to the traditional molding method, the obtained catalyst particle size distribution is wide, the particle spacing is large when the catalyst is loaded, and hot spots are easy to appear during the reaction process. Summary of the invention

[0009] In order to solve the problems that the catalyst for hydrogenating olefin aldehyde to alkanol in the prior art uses precious metals, resulting in high catalyst cost, uses metal chromium, causing environmental pollution, and the multi-step hydrogenation process is complicated and unsuitable for industrial application, the present invention provides a method for preparing 2-propyl-1-heptanol.

[0010] It is well known in the art that for an annual production of 100,000 tons of decanol, under the condition of unchanged conversion rate, the annual economic benefit can be increased by about 2 million for every 1% increase in selectivity; in addition, the reduction of by-products can reduce the energy consumption of subsequent product distillation separation, thereby achieving the purpose of energy saving, emission reduction and efficiency improvement. Therefore, in order to improve the selectivity of decanol, the present invention provides a method for preparing 2-propyl-1-heptanol, the method comprising: contacting 2-propyl-2-heptenal with hydrogen in the presence of a catalyst to cause a hydrogenation reaction;

[0011] The preparation method of the catalyst comprises: contacting alumina microspheres with a nitrogen-containing polymer solution, then first calcining the contact product under an inert atmosphere to obtain a carrier, and then loading the metal active component on the carrier.

[0012] The invention adopts specific alumina microspheres to perform carbon-nitrogen doping to obtain a carrier, and then loads a metal active component to obtain the catalyst of the invention. The catalyst of the invention adopts a one-step hydrogenation method to hydrogenate 2-propyl-2-heptenal to prepare 2-propyl-1-heptanol without using precious metals and metallic chromium, and obtains a higher 2-propyl-2-heptenal conversion rate and 2-propyl-1-heptanol selectivity. DETAILED DESCRIPTION

[0013] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0014] In the present invention, unless otherwise specified, the diameter of alumina microspheres refers to the average diameter of alumina microspheres.

[0015] The present invention provides a method for preparing 2-propyl-1-heptanol, the method comprising: in the presence of a catalyst, contacting 2-propyl-2-heptenal with hydrogen to cause a hydrogenation reaction;

[0016] The preparation method of the catalyst comprises: contacting alumina microspheres with a nitrogen-containing polymer solution, then first calcining the contact product under an inert atmosphere to obtain a carrier, and then loading the metal active component on the carrier.

[0017] According to the present invention, preferably, the particle diameter of the alumina microspheres is 200-800 μm, and the coefficient of variation is 3-8%.

[0018] According to the present invention, the source of the alumina microspheres is not particularly limited, as long as the particle diameter and coefficient of variation of the alumina microspheres meet the specified range. The alumina microspheres can be prepared by referring to the method described in CN110203953B or CN110282642B. Preferably, the preparation method of the alumina microspheres comprises: using aluminum sol as a dispersed phase and an organic solvent as a continuous phase, forming droplets of the dispersed phase under the shearing action of the continuous phase, obtaining gel microspheres by solidification, and then obtaining alumina microspheres by drying and calcining.

[0019] In the method for preparing alumina microspheres according to the present invention, preferably, the aluminum sol has a solid content of 5-8 wt %.

[0020] In the method for preparing alumina microspheres according to the present invention, preferably, the organic solvent used in the process of preparing alumina microspheres is a C1-C10 monohydric saturated alcohol, preferably octanol.

[0021] In the method for preparing alumina microspheres according to the present invention, the drying temperature may be 100-120° C., and the drying time may be 3-15 hours.

[0022] In the method for preparing alumina microspheres according to the present invention, the calcination temperature may be 550-1200° C., and the calcination time may be 4-10 hours.

[0023] According to the present invention, preferably, the alumina microspheres are prepared in a microchannel reactor. There is no particular limitation on the type of the microchannel reactor, and the microchannel reactor is a single-channel reactor and / or a multi-channel reactor.

[0024] According to a further preferred embodiment of the present invention, the multi-channel reactor is an eight-channel reactor. The structure of the eight-channel reactor is described, and the eight-channel reactor includes a continuous phase distribution layer, a first droplet generation layer, a second droplet generation layer and a dispersed phase distribution layer, wherein the continuous phase distribution layer is composed of a petal-shaped resistance distribution channel and eight fluid outlets at its end, a continuous phase vertical inlet and four positioning holes, each branch of the fluid passing through is called a level, and a certain resistance is added before each level of fluid branch, and the width of the channel decreases as the radius of the circle where the starting end of each level is located increases; the first droplet generation layer is distributed with eight T-shaped channels, four positioning holes and eight through holes to meet the needs of the continuous phase flowing from the distribution layer to the generation layer, the second droplet generation layer is similar to the first droplet generation layer in structure, and eight droplet outlets are distributed at the end of the main channel of the T-shaped channel; the dispersed phase distribution layer is similar to the continuous phase distribution layer in structure, except for the petal-shaped resistance distribution channel and the eight dispersed phase outlets at its end, there is also a dispersed phase fluid inlet and 8 product outlets.

[0025] According to the present invention, preferably, an eight-channel reactor is used as an example to illustrate the process of preparing alumina microspheres of the present invention. Alumina sol is used as a dispersed phase, an organic solvent is used as a continuous phase, the flow rate of the continuous phase is adjusted, the continuous phase fills the continuous phase distribution layer and flows into the droplet generation layer, and then flows out from the outlet, the continuous phase flow rate is finally stabilized at 6-10mL / min, the dispersed phase flow rate is adjusted to 1-4mL / min, the dispersed phase fills the dispersed phase distribution layer and flows into the droplet generation layer, and droplets are further generated under the shearing action of the continuous phase, and the droplets are solidified in the oil column to obtain gel microspheres, which are dried and calcined to obtain alumina microspheres with a diameter of 200-800μm and a coefficient of variation of 3-8%.

[0026] According to the present invention, the amount of the nitrogen-containing polymer can be selected within a wide range. Preferably, the amount of the nitrogen-containing polymer solution is 0.1-1 g relative to 100 g of alumina microspheres.

[0027] According to the present invention, the contact conditions between the alumina microspheres and the nitrogen-containing polymer solution can be selected within a wide range. Preferably, the contact temperature is 100-120° C. and the contact time is 4-10 h.

[0028] According to the present invention, the type of the nitrogen-containing polymer can be selected within a wide range. Preferably, the nitrogen-containing polymer in the nitrogen-containing polymer solution is a polymer containing a nitrogen heterocycle, preferably at least one of polyvinyl imidazole, polyvinyl pyridine and polyvinyl pyrrolidone, more preferably polyvinyl imidazole.

[0029] According to the present invention, the concentration of the nitrogen-containing polymer in the nitrogen-containing polymer solution is not particularly limited. Preferably, the concentration of the nitrogen-containing polymer in the nitrogen-containing polymer solution is 0.1-1wt%. (For example, it can be 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%).

[0030] According to the present invention, preferably, the solvent used in the process of preparing the nitrogen-containing polymer solution is an alcohol, preferably a C1-C4 saturated alcohol, more preferably methanol and / or ethanol.

[0031] According to the present invention, the conditions for the first calcination can be selected within a wide range. Preferably, the temperature of the first calcination is 400-800° C. and the time is 2-10 h.

[0032] According to the present invention, preferably, the method for preparing the catalyst further comprises first drying the product of the contact between the alumina microspheres and the nitrogen-containing polymer solution and then first calcining it. More preferably, the temperature of the first drying is 60-80°C and the time is 4-12h.

[0033] According to the present invention, preferably, the metal active component is Ni.

[0034] According to the present invention, preferably, the amount of the metal active component used is 5-20 g in terms of metal element relative to 20 g of the carrier.

[0035] According to the present invention, preferably, the amount of the metal active component used is such that the content of the metal active component in the obtained catalyst, calculated as the metal element, is 15-50 wt %.

[0036] According to the present invention, preferably, the metal active component is loaded on the carrier by impregnating the carrier with an impregnation solution containing the metal active component, and then performing a second calcination under an inert atmosphere.

[0037] According to the present invention, preferably, the impregnation solution containing metal active components is prepared by dissolving a water-soluble salt of a metal in water. More preferably, the mass percentage of the metal in the impregnation solution containing metal active components is 10-15wt%.

[0038] According to the present invention, the conditions for the impregnation with the impregnation liquid can be selected within a wide range. Preferably, the impregnation temperature is 30-40° C. and the time is 1-5 h.

[0039] In the present invention, the impregnation method can be any of the impregnation methods commonly used in the art, such as equal volume impregnation method, excess impregnation method, and can be a single impregnation or multiple impregnations, as long as the loading amount of the metal active component can meet the requirements.

[0040] According to the present invention, the conditions for the second calcination can be selected within a wide range. Preferably, the temperature of the second calcination is 300-600° C. and the time is 4-8 hours.

[0041] According to the present invention, preferably, the method for preparing the catalyst further comprises subjecting the impregnated carrier to a second drying followed by a first calcination. More preferably, the second drying is carried out at a temperature of 80-120° C. for a time of 4-12 h.

[0042] According to the present invention, preferably, the conditions of the hydrogenation reaction include: a temperature of 50-200°C, preferably 90-150°C, a hydrogen pressure of 0.5-8MPa, preferably 3-5MPa, a liquid hourly mass space velocity of 2-propyl-2-heptenal of 0.01-5h -1 , preferably 0.02-0.1h -1 .

[0043] According to the present invention, preferably, the 2-propyl-2-heptenal is contacted with hydrogen in the form of a 2-propyl-2-heptenal solution, and the solvent in the 2-propyl-2-heptenal solution is a C1-C10 saturated alcohol.

[0044] According to the present invention, preferably, the molar ratio of the 2-propyl-2-heptenal to hydrogen is 1:50-100.

[0045] According to the present invention, preferably, the weight ratio of the 2-propyl-2-heptenal to the C1-C10 saturated alcohol is 1:5-10.

[0046] According to the present invention, preferably, the C1-C10 saturated alcohol is decanol.

[0047] The present invention will be described in detail below by way of examples. In the following examples,

[0048] Decenal conversion rate = (the number of moles of decenal in the raw material - the number of moles of unreacted decenal) ÷ ​​the number of moles of decenal in the raw material × 100%.

[0049] Decyl alcohol selectivity = the number of moles of decanol in the product ÷ (the number of moles of decenal in the raw material - the number of moles of unreacted decenal) × 100%.

[0050] The diameter of alumina microspheres was measured by scanning electron microscopy.

[0051] The test method of the coefficient of variation is as follows: the number of alumina microspheres in a unit area is measured by scanning electron microscopy, and the diameter of each alumina microsphere is measured, and then the coefficient of variation is calculated according to the formula.

[0052] The coefficient of variation was calculated according to the following formula:

[0053]

[0054] CV: coefficient of variation, n: alumina microsphere particle count, X i : single alumina microsphere particle diameter, The average particle diameter of all alumina microspheres.

[0055] Preparation Example

[0056] Alumina microspheres were prepared using a microstructured reactor. The dispersed phase was aluminum sol with a solid content of 7.5wt%, and the continuous phase and the liquid in the oil column were organic solvent octanol. The continuous phase flow rate was first adjusted so that the continuous phase filled the continuous phase distribution layer and flowed into the droplet generation layer, and then flowed out from the outlet. The continuous phase flow rate was finally stabilized at 6-10mL / min. Then the dispersed phase flow rate was adjusted to 1-4mL / min, so that the dispersed phase filled the dispersed phase distribution layer and flowed into the droplet generation layer, and droplets were further generated under the shearing action of the continuous phase. The droplets solidified in the oil column to obtain gel microspheres, which were dried at 120°C for 12 hours and calcined at 600°C for 4 hours to obtain alumina microspheres with a diameter of 345μm and a coefficient of variation of 7.2%.

[0057] Example 1

[0058] (1) 100 g of the alumina microspheres obtained in the preparation example were immersed in an ethanol solution of polyvinyl imidazole with a concentration of 1 wt% (wherein the amount of polyvinyl imidazole was 1 g), and then transferred to a hydrothermal autoclave to react at 100° C. for 10 h, cooled and filtered, dried at 80° C. for 4 hours, and then placed in a nitrogen atmosphere and calcined at 400° C. for 10 hours to obtain a carrier (carbon-doped alumina microspheres).

[0059] (2) 20 g of the carrier was placed in a 15 wt % nickel nitrate aqueous solution (wherein the amount of nickel nitrate calculated as the metal element was 5 g), and the carrier was taken out after being immersed at 30° C. for 5 h, drained, dried at 80° C. for 12 h, and calcined at 600° C. for 4 h in a nitrogen atmosphere to obtain a catalyst.

[0060] X-ray fluorescence spectroscopy (XRF) analysis showed that the nickel loading in the catalyst was 18.9 wt %.

[0061] Example 2

[0062] Step (1) is the same as in Example 1.

[0063] (2) 20 g of the carrier was placed in a 15 wt % nickel nitrate aqueous solution (wherein the amount of nickel nitrate calculated as the metal element was 5 g), and the carrier was taken out after being immersed at 30° C. for 5 h, drained, dried at 80° C. for 12 h, and calcined at 600° C. for 4 h in a nitrogen atmosphere.

[0064] (3) Repeat step (2) three times to obtain a catalyst.

[0065] XRF characterization showed that the nickel loading in the catalyst was 43.7 wt%.

[0066] Example 3

[0067] (1) 100 g of the alumina microspheres obtained in the preparation example were immersed in an ethanol solution of polyvinyl imidazole with a concentration of 0.1 wt% (wherein the amount of polyvinyl imidazole was 0.1 g), and then transferred to a hydrothermal autoclave for reaction at 120° C. for 4 h, cooled and filtered, dried at 60° C. for 12 h, and then placed in a nitrogen atmosphere and calcined at 800° C. for 2 h to obtain a carrier (carbon-doped alumina microspheres).

[0068] (2) 20 g of the carrier was placed in a 15 wt % nickel nitrate aqueous solution (wherein the amount of nickel nitrate calculated as the metal element was 5 g), immersed at 40° C. for 1 h, then the carrier was taken out, drained, dried at 120° C. for 4 hours, and calcined at 300° C. in a nitrogen atmosphere for 8 hours.

[0069] (3) Repeat step (2) three times to obtain a catalyst.

[0070] XRF characterization showed that the nickel loading in the catalyst was 44.7 wt%.

[0071] Comparative Example 1

[0072] The catalyst was prepared according to the method of Example 1, except that the carrier was replaced with alumina balls (purchased from Inokai Biotechnology Co., Ltd., with a particle size of 3-4 mm).

[0073] XRF characterization showed that the nickel loading in the catalyst was 19.5 wt%.

[0074] Comparative Example 2

[0075] The catalyst was prepared according to the method of Example 2, except that the carrier was replaced with alumina balls (purchased from Inokai Biotechnology Co., Ltd., with a particle size of 3-4 mm).

[0076] XRF characterization showed that the nickel loading in the catalyst was 45.3 wt%.

[0077] Comparative Example 3

[0078] The catalyst was prepared according to the method of Example 1, except that the process of preparing the carrier in step (1) was not included, that is, alumina microspheres were directly used as the carrier.

[0079] XRF characterization showed that the nickel loading in the catalyst was 19.7 wt%.

[0080] Test Case

[0081] The performance of the catalysts of the above embodiments and comparative examples in preparing 2-propyl-1-heptanol by liquid phase hydrogenation of 2-propyl-2-heptenal was tested. 20 mL of the catalyst was loaded into a reactor. After reduction at 450° C. for 4 h in a hydrogen atmosphere, hydrogen, liquid 2-propyl-2-heptenal and solvent (2-propyl-1-heptanol) were continuously fed. The reaction temperature, hydrogen pressure, liquid hourly weight space velocity of 2-propyl-2-heptenal and weight ratio of 2-propyl-2-heptenal to solvent are shown in Table 1. The test results are shown in Table 1.

[0082] Table 1

[0083]

[0084]

[0085] Note: Decenal in Table 1 refers to 2-propyl-2-heptenal.

[0086] It can be seen from the results in Table 1 that the catalyst prepared by the method of the present invention has a higher 2-propyl-2-heptenal conversion rate and a higher 2-propyl-1-heptenal selectivity when used for preparing 2-propyl-2-heptenal by liquid phase hydrogenation of 2-propyl-2-heptenal. Comparing Comparative Example 1-2 with Example 1-3, the metal active component content in the catalyst is substantially the same, and under the same hydrogenation test conditions, the catalyst of Example 1-3 can further improve the selectivity of 2-propyl-1-heptenal while ensuring the conversion rate of 2-propyl-2-heptenal, and the selectivity is improved by more than 1%.

[0087] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing 2-propyl-1-heptanol, characterized in that: The method comprises: in the presence of a catalyst, contacting 2-propyl-2-heptenal with hydrogen to cause a hydrogenation reaction; The preparation method of the catalyst comprises: contacting alumina microspheres with a nitrogen-containing polymer solution, then first calcining the contact product under an inert atmosphere to obtain a carrier, and then loading a metal active component on the carrier, wherein the nitrogen-containing polymer in the nitrogen-containing polymer solution is polyvinyl imidazole, and the metal active component is Ni.

2. The method according to claim 1, wherein: The amount of the nitrogen-containing polymer solution used is 0.1-1 g, calculated as the nitrogen-containing polymer, relative to 100 g of alumina microspheres.

3. The method according to claim 1, wherein: The temperature of the contact between the alumina microspheres and the nitrogen-containing polymer solution is 100-120° C. and the time is 4-10 hours.

4. The method according to claim 1, wherein: The diameter of the alumina microspheres is 200-800 μm, and the coefficient of variation is 3-8%; and / or, the concentration of the nitrogen-containing polymer in the nitrogen-containing polymer solution is 0.1-1 wt %; And / or, the solvent used in the process of preparing the nitrogen-containing polymer solution is alcohol.

5. The method according to claim 1, wherein: The solvent used in the process of preparing the nitrogen-containing polymer solution is a C1-C4 saturated alcohol.

6. The method according to claim 1, wherein: The solvent used in the process of preparing the nitrogen-containing polymer solution is methanol and / or ethanol.

7. The method according to claim 1, wherein: The temperature of the first calcination is 400-800° C., and the time is 2-10 hours.

8. The method according to claim 1, wherein: The amount of the metal active component used is 5-20 g in terms of metal element relative to 20 g of the carrier.

9. The method according to claim 1, wherein: The method of loading the metal active component on the carrier is to use an impregnation solution containing the metal active component to impregnate the carrier, and then perform a second calcination under an inert atmosphere.

10. The method according to claim 9, wherein: The immersion temperature is 30-40°C and the immersion time is 1-5h.

11. The method according to claim 9, wherein: The second calcination is carried out at a temperature of 300-600° C. and for a time of 4-8 hours.

12. The method according to claim 1, wherein: The conditions of the hydrogenation reaction include: a temperature of 50-200°C, a hydrogen pressure of 0.5-8 MPa, a liquid hourly mass space velocity of 2-propyl-2-heptenal of 0.01-5 h -1 .

13. The method according to claim 1, wherein: The temperature of the hydrogenation reaction is 90-150°C.

14. The method according to claim 1, wherein: The conditions of the hydrogenation reaction include: the hydrogen pressure is 3-5 MPa.

15. The method according to claim 1, wherein: The conditions of the hydrogenation reaction include: the liquid hourly mass space velocity of 2-propyl-2-heptenal is 0.02-0.1h -1 .

16. The method according to claim 1, wherein: The 2-propyl-2-heptenal is contacted with hydrogen in the form of a 2-propyl-2-heptenal solution, wherein the solvent in the 2-propyl-2-heptenal solution is a C1-C10 saturated alcohol; And / or, the molar ratio of 2-propyl-2-heptenal to hydrogen is 1:50-100.

17. The method according to claim 16, wherein: The weight ratio of the 2-propyl-2-heptenal to the C1-C10 saturated alcohol is 1:5-10; And / or, the C1-C10 saturated alcohol is decanol.