A fully bio-based degradable composite material
Polymers and starch were solved by using all-biomaterial composites such as glycol glycidyl ether in polylactic acid, polyadipic acid/butylene terephthalate, polycaprolactone and starch The problem of poor compatibility between the two significantly improves the toughness and application range of composite materials.
Patent Information
- Application Number
- CN202310196587.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-17
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-02
AI Technical Summary
In the prior art, hydrophobic polymers such as polylactic acid, polycaprolactone, polyadipic acid/butylene terephthalate have poor compatibility, and starch plasticization and coupling agent modification cause polymers and The problem of degradation of mechanical properties of starch composites.
Polylactic acid, polyadipic acid/butylene terephthalate, polycaprolactone and starch are used as raw materials, and ethylene glycol glycidyl ether, glycerol triglycidyl ether and pentaerythritol glycidyl ether are added as capacity enhancement Agent, the preparation of fully biomassed degradable composite materials by melt blending, improves the interface compatibility and mechanical properties between polymer and starch.
It significantly improves the toughness of composite materials, up to 400% to 500%, improves the interface compatibility of polymer/starch composite materials, and expands the application range of degradable materials.
Smart Images

Figure CN116041925B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of degradable materials, and more specifically, to a fully bio-based degradable composite material. Background Art
[0002] Plastic is the most common polymer material in people's lives. As one of them, petroleum-based plastic is difficult to degrade and incineration pollutes the atmosphere, so its use is restricted. Using biodegradable polymer materials to replace petroleum-based plastics has become a global development trend. Common biodegradable materials include polylactic acid, polybutylene adipate / terephthalate and polycaprolactone. For example, polylactic acid (PLA) is a linear aliphatic polyester with good mechanical strength, easy processing and high transparency. Polybutylene adipate / terephthalate (PBAT) is a biodegradable elastomer with good ductility and elongation at break, as well as good heat resistance and impact resistance. Polycaprolactone (PCL) is a semi-crystalline thermoplastic plastic with good flexibility, melt strength and biocompatibility. However, there are obvious performance defects between the three individually, which limits their application. Due to the large performance differences and poor compatibility between the three, it is often difficult to mix and apply them at the same time.
[0003] For the common compatibilizers on the market used to improve PLA and other plastics such as PBAT and PCL, such as isocyanate compatibilizers, the toxicity of the isocyanate group makes this type of compatibilizer unable to be used in the food industry; oxazoline compatibilizers are difficult to be widely used due to their high prices; and for common epoxy compatibilizers, such as epoxidized soybean oil, there are problems such as low epoxy value and poor reactivity, resulting in poor compatibilization effect.
[0004] In addition, starch (ST), as a cheap, renewable and biodegradable polymer material, can be used as an organic filler for degradable bioplastics, which can greatly reduce the cost of degradable polymer-based products and is an important development direction in the future. However, because starch has an intermolecular and intramolecular hydrogen bond network, it is a hydrophilic material, while polylactic acid and polylactone are hydrophobic materials, and the two are thermodynamically incompatible. And because starch has a rigid granular structure with a particle size range of 10 to 200 μm, when starch is blended with PLA, it will cause severe stress concentration, which will further reduce the strength and toughness of the composite material. In order to improve the compatibility between polymers and starch and improve the performance of the mixture, there are generally two commonly used methods: the first is to plasticize starch, and the strong hydrogen bonds in starch are destroyed by using small molecule plasticizers to obtain hydrophobic thermoplastic starch TPS. Commonly used plasticizers include water, glycerol, formamide and sorbitol. However, small molecule plasticizers may cause PLA to degrade during processing. Moreover, TPS containing a small amount of plasticizers is an unstable system because these small-molecule plasticizers react with starch particles only through hydrogen bonds and can easily migrate out of the TPS matrix over time, eventually causing the starch in TPS to retrograde, which may cause the mechanical properties of the polymer / starch composites to deteriorate again.
[0005] Another method is to use a coupling agent to improve the interfacial compatibility between the polymer matrix and starch. A coupling agent containing a reactive functional group, such as a maleic anhydride group, an isocyanate group, etc., is used, such as CN202010050189.0 A fully bio-based degradable polymer / starch composite material and a preparation method thereof discloses that the fully bio-based degradable polymer / starch composite material includes 70-95wt% polylactic acid and 5-30wt% grafted modified starch, and the grafted modified starch includes furfuryl glycidyl ether grafted starch. Among them, the furfuryl glycidyl ether grafted starch is obtained by reacting starch with maleic anhydride to obtain maleic anhydride grafted starch, and then grafting and modifying it with furfuryl glycidyl ether. However, the functionalization of PLA by the above-mentioned coupling agent is very low, the reaction is difficult to carry out, and the process of using the above-mentioned coupling agent is complicated, the cost is high, and it is difficult to industrialize. Some researchers have also used natural vegetable oils, such as epoxidized soybean oil, epoxidized sesame oil, etc., to utilize epoxy groups to react with hydroxyl groups on PLA and starch to achieve the effect of volume expansion. Although the flexible oil layer attached to the interface between the two phases can enhance the toughness of the PLA / ST composite material, it will lead to a significant reduction in the strength of the composite material. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a fully bio-based degradable composite material in view of the poor compatibility between hydrophobic polymers such as polylactic acid, polycaprolactone, and polybutylene adipate / terephthalate in the prior art, and the reduction of mechanical properties of polymer and starch composite materials caused by starch plasticization and coupling agent modification.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A fully bio-based degradable composite material, characterized in that the raw materials include at least two of polylactic acid, polybutylene adipate / terephthalate, polycaprolactone and starch, and the content of one substance in the raw materials is not less than 50wt.% in mass percentage; a compatibilizer is added to the raw materials, and the added amount is 1-20% of the total mass of the raw materials; the compatibilizer is one or more of ethylene glycol glycidyl ether, propylene glycol triglycidyl ether and pentaerythritol glycidyl ether.
[0009] Furthermore, the raw material components include 50-85wt.%, polylactic acid, 0-30wt.%, polybutylene adipate / terephthalate, 0-30wt.%, polycaprolactone, 0-50wt.%, starch, and the added amount of the compatibilizer is 1-5% of the total mass of the raw material components.
[0010] Preferably, the raw material components include 85 wt.% of polylactic acid and 15 wt.% of starch. The compatibilizer is glycerol triglycidyl ether, and the added amount thereof is 3% of the total mass of the polylactic acid and starch.
[0011] Preferably, the raw material components include 50wt.%, polylactic acid, 25wt.%, polycaprolactone, and 25wt.% starch; the compatibilizer is propylene triglycidyl ether, and its addition amount is 3% of the total mass of polylactic acid, polycaprolactone, and starch; the catalyst is triethylamine, and its addition amount is 0.4% of the total mass of polylactic acid, polycaprolactone, and starch.
[0012] Preferably, the raw material components include 70wt.%, polylactic acid, 15wt.%, polybutylene adipate / terephthalate, and starch, and the compatibilizer is ethylene glycol glycidyl ether, and its added amount is 3% of the total mass of polylactic acid, polybutylene adipate / terephthalate and starch.
[0013] Preferably, the raw material components include 70 wt.% of polylactic acid and 30 wt.% of polybutylene adipate / terephthalate, and the compatibilizer is propylene glycol triglycidyl ether, and the added amount thereof is 3% of the total mass of polylactic acid and polybutylene adipate / terephthalate.
[0014] Preferably, the raw material components include 70 wt.% of polylactic acid and 30 wt.% of polycaprolactone. The compatibilizer is glycerol triglycidyl ether, and the added amount thereof is 3% of the total mass of polylactic acid and polycaprolactone.
[0015] Preferably, the raw material components include 85 wt.% of polylactic acid and 15 wt.% of polycaprolactone. The compatibilizer is glycerol triglycidyl ether, and the added amount thereof is 5% of the total mass of polylactic acid and polycaprolactone.
[0016] Furthermore, the raw material also includes a catalyst, and the catalyst is a basic tertiary amine, including one or more of triethylamine, tributylamine, trimethylamine, dodecyldimethylamine, and hexadecyldimethylamine.
[0017] Furthermore, the raw material components include 70wt.% of polycaprolactone, 30wt.% of starch, the compatibilizer is glycerol triglycidyl ether, and its addition amount is 2% of the total mass of polycaprolactone and starch, and the catalyst is triethylamine, and its addition amount is 0.5% of the total mass of polycaprolactone and starch.
[0018] Furthermore, the starch is natural starch that has not been plasticized and modified, including one or more of corn starch, tapioca starch, wheat starch, potato starch, and sweet potato starch.
[0019] Furthermore, the raw materials of the all-biobased degradable polymer / starch composite material also include modifiers and processing aids, and the modifiers and processing aids are one or more of toughening agents, plasticizers, thermal stabilizers, lubricants, nucleating agents, flame retardants and colorants.
[0020] Furthermore, the addition amount of the modifier and processing aid is 0.05-20% of the total mass of the polymer and starch.
[0021] Furthermore, the toughening agent is a thermoplastic polyester elastomer, a polyamide elastomer or a polyester ether elastomer.
[0022] Furthermore, the plasticizer is one or more of aliphatic dibasic acid esters, phosphate esters, epoxy compounds, polyol esters, polyethers and polyester plasticizers.
[0023] Furthermore, the heat stabilizer is phosphite and phenolic antioxidant.
[0024] Furthermore, the lubricant is one or more of polyethylene oxide, stearic acid, C12-C18 alcohol, epoxidized soybean oil or epoxidized stearate.
[0025] Furthermore, the nucleating agent is one or more of organic carboxylates such as sodium butyrate and sodium methylvalerate, sulfonates and inorganic silicate silica gel, talc, carbonates and phosphates.
[0026] Furthermore, the preparation steps of the all-biobased degradable polymer / starch composite material include: drying the raw materials, mixing them evenly with a compatibilizer, a modifier and a processing aid according to a ratio, then melt-blending, extruding and granulating them at 180-220°C, and drying them to obtain the all-biobased degradable polymer / starch composite material.
[0027] Furthermore, the moisture content of the raw polymer is controlled to be less than 0.5%, and the moisture content of the starch is controlled to be less than 1.0%.
[0028] Furthermore, the all-biobased degradable composite material is applied to packaging materials, disposable containers, disposable cutlery, forks and spoons, ground films, instruments and medical products.
[0029] Compared with the prior art, the beneficial effects are:
[0030] The present invention uses ethylene glycol glycidyl ether (EGDE), glycerol triglycidyl ether (GTE) and pentaerythritol glycidyl ether (PGE) as compatibilizers of a fully bio-based degradable composite material in a system of fully degradable materials of polylactic acid, polyadipate / butylene terephthalate, polycaprolactone and starch, and obtains a bio-based degradable composite material with excellent comprehensive performance through melt blending. In the present invention, by adding a small amount of compatibilizer, the toughness of the composite material can be significantly improved, and the maximum increase can be 400% to 500%, which greatly expands the application of degradable materials. In addition, starch (ST) is added to the polymer as a filler, and the epoxy group on the compatibilizer reacts with the polymer and the hydroxyl group on the ST, thereby improving the interface compatibility of the polymer / starch composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the SEM image of the PLA / ST composite material in Example 2;
[0032] Among them, a is pure PLA, b is EGDE-0, c is EGDE-3, d is GTE-3, and e is PGE-3
[0033] Figure 2 Graph showing tensile strength and elongation at break of PLA / ST composite materials with different contents of compatibilizer in Example 2;
[0034] Figure 3 DSC graphs of pure PLA, PLA / ST composites without and with 3% compatibilizer added in Example 2;
[0035] Figure 4 is the infrared spectrum of the eluted starch in Example 3;
[0036] Figure 5is a SEM photo of the PLA / ST composite material prepared in Example 3;
[0037] Among them, a is GTE-0, b is GTE-1, c is GTE-2, d is GTE-3, e is GTE-4, f is EGDE-3, and g is PGE-3;
[0038] Figure 6 Han diagrams of pure PLA, PLA without addition, and PLA with different compatibilizers in Example 3.
[0039] Figure 7 Graphs showing tensile strength and elongation at break of pure PLA, PLA without adding or adding different compatibilizers in Example 3;
[0040] Figure 8 DSC graphs of pure PLA and PLA / ST composites with different compatibilizer contents in Example 3;
[0041] Fig. 9 Graph showing tensile strength and elongation at break of the PLA / ST composite material sample in Example 4;
[0042] Fig.10 Graph showing tensile strength and elongation at break of the PLA / ST composite material sample in Example 5;
[0043] Fig.11 Graph showing the tensile strength and elongation at break of the PCL / ST composite material sample in Example 6;
[0044] Fig.12 Graph showing tensile strength and elongation at break of the PLA / PCL / ST composite material sample in Example 7;
[0045] Fig.13 Graph showing tensile strength and elongation at break of the PLA / PBAT / ST composite material sample in Example 8;
[0046] Fig.14 Graph showing tensile strength and elongation at break of the PLA / PBAT composite material sample in Example 9;
[0047] Fig.15 Graph showing tensile strength and elongation at break of the PLA / PCL composite material sample in Example 10;
[0048] Fig.16 This is a graph of the tensile strength and elongation at break of the PLA / PCL composite material sample in Example 11. DETAILED DESCRIPTION
[0049] The following is further explained and illustrated in conjunction with the examples, but the specific examples do not limit the present invention in any form. If not specifically stated, the methods and equipment used in the examples are conventional methods and equipment in the art, and the raw materials used are all conventional commercially available raw materials.
[0050] Example 1
[0051] This embodiment provides a method for preparing a fully bio-based degradable polymer / starch composite material, the steps comprising: taking a certain amount of polymer and corn starch for drying, controlling the polymer moisture content to be less than 0.5%, and the starch moisture content to be less than 1.0%. Then, the polymer, corn starch and compatibilizer are mixed in a high-speed mixer at room temperature at 1000 rpm for 10 minutes, and then the obtained mixture is melt-blended and extruded into granules in a twin-screw extruder at 180-220°C, and dried to obtain a fully bio-based degradable polymer / starch or polymer / polymer composite material. -
[0052] Example 2
[0053] According to the method described in Example 1, this example uses polylactic acid as the polymer matrix, and different contents of compatibilizers are set to obtain a fully bio-based degradable polymer / starch composite material. The content of the components is shown in Table 1 below, and the materials obtained in Table 1 are subjected to electron microscopy scanning, mechanical properties testing, crystallization properties and other tests.
[0054] Table 1
[0055] PLA / wt% ST / wt% EGDE / wt% GTE / wt% PGE / wt% Pure PLA 100 0 0 0 0 EGDE-0 85 15 0 0 0 EGDE-0.5 85 15 0.5 0 0 EGDE-1 85 15 1 0 0 EGDE-2 85 15 2 0 0 EGDE-3 85 15 3 0 0 GTE-0.5 85 15 0 0.5 0 GTE-1 85 15 0 1 0 GTE-2 85 15 0 2 0 GTE-3 85 15 0 3 0 GTE-4 85 15 0 4 0 PGE-0.5 85 15 0 0 0.5 PGE-1 85 15 0 0 1 PGE-2 85 15 0 0 2 PGE-3 85 15 0 0 3
[0056] like Figure 1 As shown in the scanning electron microscope image, the cross section of pure PLA is smooth. After adding 15% starch, a large number of starch granules can be seen to be enriched in the PLA matrix, and the interface between PLA and ST is smooth with large gaps, indicating that the interface compatibility between the two is poor. After adding 3% EGDE, GTE and PGE respectively, it can be clearly seen that the starch granules are evenly dispersed in the PLA matrix, the interface between the two phases is blurred, the gap is reduced, and some starch granules are wrapped by the PLA matrix, which indicates that the compatibility of PLA and starch is improved after adding the three compatibilizers respectively.
[0057] like Figure 2As shown in the tensile strength and elongation at break graph, the tensile strength of pure PLA is about 71.8MPa, and the elongation at break is about 6%. After adding 15% starch, the mechanical properties of the composite material decreased significantly, and the tensile strength and elongation at break were only 56.7MPa and 4.1%, respectively. This is mainly due to the thermodynamic incompatibility between PLA and starch. After adding the compatibilizers EGDE, GTE and PGE, it can be seen that the mechanical properties have been improved, and the optimal amount of the compatibilizer is between 2% and 3%, which is due to the compatibility improving the interfacial adhesion of the PLA / ST composite material.
[0058] As shown in Table 2 and Figure 3 The DSC data of the composite material shown in the graph shows that the Tg of pure PLA is around 63°C and the crystallinity is 9%. After adding starch, the crystallinity decreases. This may be because the larger starch particles hinder the flow of PLA molecular chains. After adding the compatibilizer, the crystallinity of the composite material is improved. This is because the compatibilizer improves the dispersion of starch particles in the PLA matrix and plays a role in improving the interfacial compatibility.
[0059] Table 2
[0060] Sample Tg(℃) Tc(℃) △Hc(J / g) Tm(℃) △Hm(J / g) Xc(℃) PLA 63 103 -24 168 33 9 EGDE-0 63 106 -22 169 27 6 EGDE-3 60 102 -26 168 35 11 GTE-3 61 101 -23 168 37 17 PGE-3 59 104 -26 168 33 9
[0061] Example 3
[0062] According to the method described in Example 1, different contents of compatibilizers were respectively set to obtain a fully bio-based degradable polymer / starch composite material, and the contents of the components are shown in Table 3 below:
[0063] Table 3
[0064]
[0065]
[0066] The properties of the fully bio-based degradable polymer / starch composites prepared with different contents in Table 3 were tested, and the test results are as follows:
[0067] The PLA and the compatibilizer in the composite material were dissolved in chloroform, and the remaining starch was subjected to spectral detection, such as Figure 4 The FT-IR spectrum shown in the figure shows that the new strong absorption peak at 1756 cm-1 can be attributed to the carbonyl group (C=O) in the eluted starch containing the compatibilizer, compared with GTE-0 without the compatibilizer. This indicates that PLA and starch are bridged by reacting with the compatibilizer, proving that the three compatibilizers reacted with PLA and starch during the melt blending process.
[0068] Depend on Figure 5The scanning electron micrographs shown in the figure show that there is an obvious gap and severe shedding between the PLA matrix and the starch granules, indicating the incompatibility of PLA and starch ( Figure 5 a). After adding GTE to the PLA / ST blend system, the compatibility of PLA and natural starch is improved, and some interfaces between the two phases become blurred ( Figure 5 b~e). This can explain that the epoxy groups of GTE with high epoxy value react with the hydroxyl groups of polylactic acid and starch, playing a role of reactive compatibility. Moreover, the compatibility is best when the GTE content is 3%. Figure 5 d It can be clearly seen that the gap between starch particles and PLA matrix almost disappeared, the interface between the two phases became blurred, and the best interfacial adhesion was obtained. With the further increase of GTE content, it can be seen that the gap of GTE-4 is larger than that of GTE-3. This is because as the amount of GTE increases, too much GTE will be enriched between starch and PLA matrix, resulting in an increase in the distance between starch and PLA matrix, and further reducing the interfacial adhesion of the composite material.
[0069] Similarly, by Figure 5 From f to g, we can see that EGDE and PGE can also be used as good compatibilizers for PLA / ST composites.
[0070] In general, if the mixture is considered a truly homogeneous material, the slope of the Han plot in the final region is 2, and improvements in the compatibility of the mixture will result in a slope of the Han plot close to 2. Figure 6 As shown in Table 4, the slope of the Han curve obtained by fitting in the low-frequency terminal region shows that the slopes of all samples deviate from 2, indicating that the samples are incompatible or partially compatible. However, for sample GTE-3, its slope is 0.88, which is much larger than 0.44 of GTE-0, indicating that the interfacial compatibility of the composite material with the addition of 3% GTE has been improved. It can also be seen from Table 4 that the slope of the Han graph of the samples after adding the compatibilizer has been improved.
[0071] Table 4
[0072] 1% 2% 3% 4% EGDE 0.61 0.67 0.79 0.68 GTE 0.51 0.63 0.88 0.63 PGE 0.52 0.67 0.83 0.81
[0073] Similarly, by Figure 7 It can be seen that the tensile strength and elongation at break of PLA materials decrease with the addition of natural starch. After adding the compatibilizer, the tensile strength and elongation at break of the composite material are significantly improved. Figure 8From the DSC data and curves shown in Table 5, it can be seen that pure PLA exhibits a glass transition at 62°C (Tg), an exothermic cold crystallization peak at 103°C (Tc), and a melting peak (Tm) at 168°C. After adding starch, it was observed that starch granules can increase the crystallinity (Xc) from 8% to 13%, which is due to the heterotropic nucleation of starch granules in the PLA matrix. The addition of GTE increased the crystallinity of PLA / ST blends to 31% and reduced the cold crystallization temperature to 92°C. GTE plays a positive role in the crystallinity of PLA / ST blends, and the same situation also occurs in composite materials with the addition of EGDE and PGE. This is due to the increased compatibility of starch granules with the PLA matrix, which may cause lamellar rearrangement and accelerate the crystallization of the PLA matrix.
[0074] Table 5
[0075] Sample Tg(℃) Tc(℃) △Hc(J / g) Tm(℃) △Hm(J / g) Xc(℃) PLA 62 103 -26 168 33 8 GTE-0 61 104 -17 168 26 13 GTE-1 56 100 -18 167 28 15 GTE-2 58 98 -16 167 30 21 GTE-3 53 93 -15 166 30 23 GTE-4 50 92 -16 164 36 31 EGDE-3 55 95 -16 167 29 20 PGE-3 54 95 -14 166 31 26
[0076] Example 4
[0077] According to the method described in Example 1, different contents of compatibilizers were respectively set to obtain a fully bio-based degradable polymer / starch composite material, and the contents of the components are shown in Table 6 below:
[0078] Table 6
[0079] PLA / wt% ST / wt% EGDE / wt% GTE / wt% PGE / wt% PLA 100 0 0 0 0 EGDE-0 50 50 0 0 0 EGDE-1 50 50 1 0 0 EGDE-2 50 50 2 0 0 EGDE-3 50 50 3 0 0 EGDE-4 50 50 4 0 0 GTE-1 50 50 0 1 0 GTE-2 50 50 0 2 0 GTE-3 50 50 0 3 0 GTE-4 50 50 0 4 0 PGE-1 50 50 0 0 1 PGE-2 50 50 0 0 2 PGE-3 50 50 0 0 3 PGE-4 50 50 0 0 4
[0080] Depend on Fig. 9 It can be seen that after adding 50% starch, the mechanical properties of the composite material decreased significantly. The tensile strength and elongation at break of the composite material without adding a compatibilizer were only 28.9MPa and 2.1%, which was due to the poor compatibility of starch particles with the PLA matrix. After adding the compatibilizer, the tensile strength and elongation at break of the composite material were significantly improved. As the amount of GTE increased to 3%, the tensile strength and elongation at break increased to 53.4MPa and 3.51%, respectively, which was about 85% and 67% higher than GTE-0.
[0081] Example 5
[0082] According to the method described in Example 1, different contents of compatibilizers were respectively set to obtain a fully bio-based degradable polymer / starch composite material, and the contents of the components are shown in Table 7 below:
[0083] Table 7
[0084]
[0085]
[0086] Depend on Fig.10It can be seen that after adding 80% starch, the mechanical properties of the composite material dropped sharply. The tensile strength and elongation at break of the composite material without the addition of the compatibilizer were only 10.5MPa and 0.95%, which is difficult to be applied in practice. After adding the compatibilizer, the tensile strength and elongation at break of the composite material were improved to a certain extent. However, the obtained composite material is still difficult to be applied in practice.
[0087] Example 6
[0088] This embodiment is based on the method described in Example 1. This embodiment uses polycaprolactone as the polymer matrix, and adds different amounts of compatibilizers to obtain a fully bio-based degradable polymer / starch composite material. The content of the components is shown in Table 8 below:
[0089] Table 8
[0090]
[0091]
[0092] Depend on Fig.11 It can be seen that the elongation at break of pure PCL is 1860%. After adding starch, the mechanical properties of the composite material decrease rapidly. The tensile strength and elongation at break are 22.2MPa and 915%, respectively. With the addition of three compatibilizers, the performance of the composite material is improved. The best group is the one with 2% pentaerythritol glycidyl ether. After adding the catalyst triethylamine, it can be seen that the performance of the composite material is also slightly improved. This is mainly because the catalyst promotes the reaction.
[0093] Example 7
[0094] This embodiment is based on the method described in Example 1. This embodiment uses polylactic acid and polycaprolactone as polymer matrices, and sets different contents of compatibilizers to obtain a fully bio-based degradable polymer / starch composite material. The contents of the components are shown in Table 9 below:
[0095] Table 9
[0096]
[0097]
[0098] In order to combine the advantages of high strength of PLA and high toughness of PCL, PLA, PCL and starch were melt blended to prepare a ternary composite material. Fig.12It can be seen that the performance of the composite material without any compatibilizer is poor, while the performance is improved after adding the compatibilizer. The best performance group is the one with 3% propylene glycol triglycidyl ether, with a tensile strength and elongation at break of 23.5MPa and 18.9% respectively. After adding the catalyst triethylamine to the group with 2% compatibilizer addition, it can be seen that the performance of the composite material with triethylamine added is also improved.
[0099] Example 8
[0100] This embodiment is based on the method described in Example 1. This embodiment uses polylactic acid and polybutylene adipate / terephthalate as polymer matrices, and sets different contents of compatibilizers to obtain a fully bio-based degradable polymer / starch composite material. The contents of the components are shown in Table 10 below:
[0101]
[0102]
[0103] Depend on Fig.13 It can be seen that after adding the three compatibilizers, the elongation at break of the composite material is improved, while the tensile strength remains unchanged without decreasing. The best group is the one with 3% ethylene glycol glycidyl ether added.
[0104] Example 9
[0105] This embodiment is based on the method described in Example 1. This embodiment uses polylactic acid and poly(butylene adipate / terephthalate) as a blending matrix, and sets different
[0106] The content of the compatibilizer is as follows:
[0107] As shown in Table 11:
[0108] PLA / wt% PBAT / wt% EGDE / wt% GTE / wt% PGE / wt% EGDE-0 70 30 0 0 0 EGDE-3 70 30 3 0 0 GTE-1 70 30 0 1 0 GTE-3 70 30 0 3 0 GTE-5 70 30 0 5 0 PGE-3 70 30 0 0 3
[0109] Depend on Fig.14 It can be seen that when no compatibilizer is added, the elongation at break and tensile strength of the composite material are 23% and 40MPa respectively. With the addition of the compatibilizer, the elongation at break of the composite material is significantly improved. When the addition amount of the compatibilizer propylene triglycidyl ether reaches 3%, it can reach up to 135%, an increase of 480%. With the improvement of toughness, the strength of the composite material decreases.
[0110] Example 10
[0111] This embodiment is based on the method described in Example 1. This embodiment uses polylactic acid and polycaprolactone as the blending matrix, and sets different contents of compatibilizers to obtain a fully bio-based degradable polymer / polymer composite material. The content of the components is shown in Table 12 below:
[0112]
[0113]
[0114] Depend on Fig.15 It can be seen that when no compatibilizer is added, the elongation at break and tensile strength of the composite material are 17% and 38MPa respectively. With the addition of the compatibilizer, the elongation at break of the composite material is significantly improved. When the addition amount of the compatibilizer propylene triglycidyl ether reaches 3%, it can reach up to 108%, an increase of 535%. With the improvement of toughness, the strength of the composite material decreases.
[0115] Embodiment 11
[0116] This embodiment is based on the method described in Example 1. This embodiment uses polylactic acid and polycaprolactone as the blending matrix, and sets different contents of compatibilizers to obtain a fully bio-based degradable polymer / polymer composite material. The content of the components is shown in Table 13 below:
[0117] PLA / wt% PCL / wt% EGDE / wt% GTE / wt% PGE / wt% EGDE-0 85 15 0 0 0 EGDE-3 85 15 3 0 0 GTE-1 85 15 0 1 0 GTE-3 85 15 0 3 0 GTE-5 85 15 0 5 0 PGE-3 85 15 0 0 3
[0118] Depend on Fig.16 It can be seen that when no compatibilizer is added, the elongation at break and tensile strength of the composite material are 41% and 51 MPa respectively. With the addition of the compatibilizer, the elongation at break of the composite material is significantly improved. When the addition amount of the compatibilizer propylene triglycidyl ether reaches 5%, it can reach a maximum of 221%, an increase of 439%. As the toughness improves, the strength of the composite material decreases.
[0119] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A fully bio-based degradable composite material, characterized in that: In terms of mass percentage, the raw material components include 70wt.% of polylactic acid, 15wt.% of polybutylene adipate / terephthalate, and 15wt.% of starch. The amount of the compatibilizer added is 3% of the total mass of polylactic acid, polybutylene adipate / terephthalate, and starch. The compatibilizer is ethylene glycol glycidyl ether, and the starch is corn starch. The preparation steps include: drying polylactic acid, polybutylene adipate / terephthalate and corn starch, controlling the moisture content of the polymer to be less than 0.5% and the moisture content of the starch to be less than 1.0%, and then mixing the polylactic acid, polybutylene adipate / terephthalate, corn starch and the compatibilizer in a high-speed mixer at room temperature at 1000 rpm for 10 minutes, and then melt-blending and extruding the obtained mixture in a twin-screw extruder at 180-220° C. to obtain granulation, and drying to obtain a fully bio-based degradable polymer / starch composite material.
2. Application of the all-biobased degradable composite material according to claim 1 in packaging materials, disposable utensils and instrument parts.