A preparation process for heat-treatable and strengthened aluminum alloy thin-walled pipe

Through the process of extrusion treatment and multi-pass cold rolling combined with solid solution annealing, the problems of low tensile strength and yield strength of 6061-T4 aluminum alloy thin-walled pipes are solved, and grain fineness and performance improvement are achieved, satisfying aviation Requirements for thin-walled pipes.

CN116043144BActive Publication Date: 2024-11-12AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310102775.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-11-12
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

The existing 6061-T4 aluminum alloy thin-walled pipe has low tensile strength and yield strength, poor stability, and is prone to defects such as orange peel, slag, and fracture in forming processes such as bending and flattening, which cannot meet the conduits of aviation aircraft systems. Requirements.

Method used

After extrusion treatment, multiple passes of cold rolling and intermediate solid solution annealing are carried out, combined with solid solution annealing of finished products, the growth of re-crystallized grains is hindered by the solid solution water quenching heat treatment mechanism, and the fineness and strength of the grains of the pipe are improved.

Benefits of technology

The tensile strength, yield strength and elongation of the 6061-T4 aluminum alloy thin-walled pipes have been significantly improved, the comprehensive performance of the pipes has been enhanced, the orange peel and fracture phenomenon has been avoided, and the performance requirements of thin-walled pipes for aviation have been met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043144B_ABST
    Figure CN116043144B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum alloy processing, and specifically to a preparation process of an aluminum alloy thin-walled pipe that can be heat-treated and strengthened. The process comprises: extruding an aluminum alloy ingot that can be heat-treated and strengthened to obtain an extruded tube billet; surface treating the extruded tube billet; cold rolling the surface-treated extruded tube billet with a large processing rate for multiple passes to obtain a rolled tube billet; pickling the rolled tube billet; vertically performing intermediate solid solution annealing on the rolled tube billet after the pickling treatment; cold rolling the rolled tube billet after the intermediate solid solution annealing treatment with a large processing rate to obtain a target finished tube; pickling the target finished tube; performing finished solid solution annealing on the target finished tube after the pickling treatment to obtain a finished tube. The purpose of the preparation process of the aluminum alloy thin-walled pipe that can be heat-treated and strengthened is to solve the problems of poor stability and low performance indicators of the aluminum alloy thin-walled pipe that can be heat-treated and strengthened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy processing, and in particular to a preparation process of an aluminum alloy thin-wall pipe that can be strengthened by heat treatment. Background Art

[0002] At present, the aluminum alloy thin-walled pipes used in aviation at home and abroad are mainly 5XXX series and 6XXX series aluminum alloys, and the grades involved are mainly 5A02, 5A06 and 6061. The main alloying elements of 6061 aluminum alloy are magnesium and silicon, which can be strengthened by heat treatment. The tensile strength of the pipe in the artificial aging state can reach 300MPa. It has good corrosion resistance, weldability and surface treatment performance. Compared with 5A02 and 5A06 aluminum alloy pipes, 6061 aluminum alloy pipes have higher strength and better sealing performance in the connection area with pipe joints. It has been widely used as the main material of system conduits abroad. Boeing, Airbus and other civil airliners and F-22, F-35 and other fighters all use this material as fuel, environmental control, hydraulic and other system pipelines.

[0003] At present, the preparation process of existing 6061-T4 aluminum alloy thin-walled pipes is "melting → extrusion → rolling (drawing) → intermediate annealing → rolling (drawing) → solid solution natural aging". According to the diameter and wall thickness of the extruded tube billet, multiple rolling (drawing) and intermediate annealing can be performed. The intermediate annealing is stress relief or recrystallization annealing, and the heat treatment system is "300℃~450℃×20~90min, air cooling", and the final solution heat treatment system of the pipe is "500~560℃×20~60min water quenching + natural aging". The tensile strength of the 6061-T4 aluminum alloy thin-walled pipes prepared by the current process is 240~265MPa, the yield strength is 90~155MPa, the elongation is 22~30%, and the stability is not good. In the forming process such as bending, flattening, and expanding, defects such as orange peel, slag, and fracture are prone to occur. 6061-T4 aluminum alloy pipes are mainly used for civil industrial products. They have low yield strength and coarse grains. They are very likely to produce orange peel phenomenon during bending and cannot meet the requirements of thin-walled pipes for aviation aircraft system ducts.

[0004] Therefore, the inventor provides a process for preparing a heat-treatable and strengthened aluminum alloy thin-walled tube. Summary of the invention

[0005] (1) Technical issues to be solved

[0006] The embodiment of the present invention provides a preparation process of an aluminum alloy thin-walled tube that can be heat-treated and strengthened, which solves the technical problems of poor stability and low performance index of the aluminum alloy thin-walled tube that can be heat-treated and strengthened.

[0007] (2) Technical solution

[0008] The present invention provides a preparation process of a heat-treatable and strengthened aluminum alloy thin-walled pipe, comprising the following steps:

[0009] Step 1, extruding the heat-treatable and strengthened aluminum alloy ingot to obtain an extruded tube blank;

[0010] Step 2, surface treating the extruded tube blank;

[0011] Step 3, subjecting the surface treated extruded tube blank to multiple passes of high processing rate cold rolling to obtain a rolled tube blank;

[0012] Step 4, pickling the rolled tube blank;

[0013] Step 5, placing the pickled rolled tube billet vertically in a heat treatment furnace for intermediate solution annealing;

[0014] Step 6, subjecting the tube blank after the intermediate solid solution annealing treatment to at least one pass of high processing rate cold rolling, and when the target finished tube is obtained, proceed to step 7; when the target finished tube is not obtained, loop through steps 4 to 6 until the target finished tube is obtained;

[0015] Step 7, pickling the target finished pipe;

[0016] Step 8: Place the target finished pipe after pickling vertically in a heat treatment furnace for solution annealing to obtain a finished pipe.

[0017] Furthermore, in step 2, the inner and outer surfaces and end faces of the extruded tube are turned and the inner and outer surfaces are polished.

[0018] Furthermore, in step 3, the processing rate of each pass is 20-50%, and the total processing rate is 45-85%.

[0019] Furthermore, in step 5, the rolled tube billet is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-560° C., put into the furnace at the temperature, kept at the temperature for 20-60 minutes, and then water quenched.

[0020] Furthermore, in step 6, the processing rate of each pass is 20-55%, and the total processing rate is 55-95%.

[0021] Furthermore, in step 8, the finished pipe is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-580° C., put into the furnace at the temperature, kept at the temperature for 30-60 minutes, and then water quenched.

[0022] Furthermore, the outer diameter of the finished pipe is 6 to 120 mm, and the wall thickness is 0.5 to 2.5 mm.

[0023] Furthermore, the finished pipe is made of 6061-T4 aluminum alloy, with a tensile strength of 266-287 MPa, a yield strength of 135-165 MPa, and an elongation of 27.5-34.5%.

[0024] (3) Beneficial effects

[0025] In summary, the present invention adopts solution water quenching heat treatment through intermediate annealing. During the solution process, the second phase particles are dispersed and precipitated to hinder the growth of recrystallized grains. The grains of the pipe structure are obviously finer than those after stress relief annealing and recrystallization annealing, and the strength and plasticity are higher.

[0026] The process of high processing rate cold rolling → solution annealing can bring into play the role of both fine grain strengthening and precipitation strengthening mechanisms, which is beneficial to improving the comprehensive performance of the pipe; at the same time, the same type of extruded tube billet can be cold processed into aluminum alloy thin-walled pipes of different specifications, expanding the process window of thin-walled pipes. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 It is a schematic flow chart of a process for preparing a heat-treatable and strengthened aluminum alloy thin-walled pipe provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to exemplarily illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the described embodiments, and covers any modification, replacement and improvement of parts, components and connection modes without departing from the spirit of the present invention.

[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0031] At present, the reasons for the low performance of pipes on the market may be: ① the cold deformation processing rate is too low, resulting in coarse recrystallized grains; ② the improper heat treatment system causes coarse recrystallized grains in the pipe, which is easy to produce orange peel phenomenon during process performance tests such as bending; ③ the pipe still has a high degree of work hardening, resulting in fracture during process performance tests. Therefore, it is necessary to improve the existing preparation process of aluminum alloy thin-walled pipes that can be heat-treated and strengthened.

[0032] Figure 1 Schematic diagram of a process for preparing a heat-treatable and strengthened aluminum alloy thin-walled pipe according to an embodiment of the present invention. Figure 1 As shown, the process may include the following steps:

[0033] S101, extruding the heat-treatable and strengthened aluminum alloy ingot to obtain an extruded tube blank;

[0034] S102, performing surface treatment on the extruded tube blank;

[0035] S103, performing multiple passes of high-processing rate cold rolling on the surface-treated extruded tube blank to obtain a rolled tube blank;

[0036] S104, pickling the rolled tube;

[0037] S105, placing the pickled rolled tube billet vertically in a heat treatment furnace for intermediate solution annealing;

[0038] S106, subjecting the tube blank after the intermediate solid solution annealing treatment to at least one pass of high processing rate cold rolling, and when the target finished tube is obtained, proceed to step S107; when the target finished tube is not obtained, loop through steps S104 to S106 until the target finished tube is obtained;

[0039] S107, pickling the target finished pipe;

[0040] S108, placing the target finished pipe after pickling treatment vertically in a heat treatment furnace for finished product solution annealing to obtain a finished pipe.

[0041] In the above-mentioned embodiment, the aluminum alloy that can be heat-treated and strengthened includes but is not limited to 2XXX, 6XXX, and 7XXX series aluminum alloys, which are mainly used in the field of aviation materials. All the following embodiments of the present invention are described in detail using 6061-T4 aluminum alloy as an example.

[0042] The main steps of preparation are: ingot extrusion → surface treatment → cold rolling → surface treatment → solution annealing → cold rolling → surface treatment → finished product solution aging.

[0043] The present invention proposes for the first time to use solution water quenching heat treatment in the intermediate annealing treatment. During the solution process, the second phase particles are dispersed and precipitated to hinder the growth of recrystallized grains. The grains of the pipe structure are obviously finer than those after the intermediate annealing using stress relief annealing and recrystallization annealing, and the strength and plasticity are higher.

[0044] As an optional embodiment, in step 2, the inner and outer surfaces and end faces of the extruded tube are turned and the inner and outer surfaces are polished.

[0045] The above is a specific method for surface treatment of extruded tube blanks. The first surface treatment can make the surface of the tube blank smoother as a whole; the second and third surface treatments (i.e. pickling) can further remove oil stains and impurities on the surface of the tube blank.

[0046] As an optional implementation, in step 3, the processing rate of each pass is 20-50%, and the total processing rate is 45-85%. The purpose of this design is to break the raw material structure through deformation at a high processing rate, increase the number of recrystallization nuclei in the later heat treatment, that is, refine the grains.

[0047] As an optional implementation, in step 5, the rolled tube is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-560° C., put into the furnace when the temperature reaches the temperature, and then quenched with water after being kept at the temperature for 20-60 minutes.

[0048] Specifically, the intermediate solution annealing eliminates work hardening, increases the precipitation and aggregation of second phase particles in the 6061 aluminum alloy, increases the strengthening effect, and strengthens the hindrance to grain growth. This process parameter is currently only for 6061 aluminum alloy.

[0049] As an optional implementation, in step 6, the processing rate of each pass is 20-55%, and the total processing rate is 55-95%. The purpose of this design is to break the raw material structure through deformation at a high processing rate, increase the number of recrystallization nuclei in the later heat treatment, that is, refine the grains.

[0050] As an optional implementation, in step 8, the finished pipe is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-580° C., put into the furnace at temperature, kept at temperature for 30-60 minutes, and then quenched with water.

[0051] Specifically, the vertical solution aging treatment of the finished product can ensure the dimensional accuracy and structural properties of the finished pipe.

[0052] As an optional implementation, the finished pipe is made of 6061-T4 aluminum alloy, with an outer diameter of 6 to 120 mm and a wall thickness of 0.5 to 2.5 mm; its tensile strength is 266 to 287 MPa, its yield strength is 135 to 165 MPa, and its elongation is 27.5 to 34.5%.

[0053] Specifically, compared with the 6061-T4 aluminum alloy thin-walled pipe with a tensile strength of 240-265 MPa, a yield strength of 90-155 MPa, and an elongation of 22-30% prepared by the current process, the performance of the thin-walled pipe obtained by the preparation process of the present invention is greatly improved.

[0054] Example 1

[0055] A preparation process of 6061-T4 aluminum alloy thin-walled tube is as follows:

[0056] The size of the 6061 aluminum alloy ingot is medium 100×25mm. The ingot is extruded at 510℃ and the extrusion barrel temperature is 480℃. The extrusion ratio is 11, and the extruded tube is extruded into a 32×6mm extruded tube. The extruded tube is turned into 31.5×5mm, and then polished with 400# and 600# sandpaper respectively. The surface roughness is Ra3.2. The polished tube is cold rolled three times, and the cold rolling processing rate is 52% respectively. , 72%, 27%. After the first cold rolling, conventional pickling is carried out. The tube billet after conventional pickling is placed vertically in a muffle furnace for solid solution treatment at 530℃ for 60min, and then loaded into a warm furnace for water quenching. After the third rolling and conventional pickling, the finished tube is placed vertically in a muffle furnace for solid solution treatment at 580℃ for 60min, and then water quenched to obtain a Ф14×1mm heat-treatable and strengthened aluminum alloy thin-walled tube.

[0057] After sampling and analysis, the grain size of the pipe is Grade 1 in GB / T3246.2, the tensile strength is 283MPa, the yield strength is 160MPa, the elongation is 30.5%, and after the pipe is sampled for bending, expansion and flattening tests, there are no cracks or orange peel phenomenon on the inner and outer surfaces.

[0058] Example 2

[0059] A preparation process of 6061-T4 aluminum alloy thin-walled tube is as follows:

[0060] The size of the 6061 aluminum alloy ingot is 100×25mm. The ingot is extruded at 510℃ and the extrusion barrel temperature is 480℃. The extrusion ratio is 11, and the extruded tube is extruded into a 32×6mm tube. The extruded tube is turned into 31.5×5mm, and then polished with 400# and 600# sandpaper respectively. The surface roughness is Ra3.2. The polished tube is cold rolled for 6 times, and the cold rolling processing rate is 52%, 59%, 2 6%, 34%, 26%, 25%, conventional pickling is carried out after the first cold rolling, the tube billet after conventional pickling is placed vertically in a muffle furnace for solid solution treatment at 530℃ for 60min, and then put into a warm furnace for water quenching; the finished tube is rolled and conventionally pickled for the 6th pass, and the finished tube is placed vertically in a muffle furnace for solid solution treatment at 540℃ for 60min, and then water quenched to obtain a Ф8×1mm heat-treatable and strengthened aluminum alloy thin-walled tube.

[0061] After sampling and analysis, the grain size of the 6061-T4 aluminum alloy pipe is Grade 1 in GB / T3246.2, the tensile strength is 258MPa, the yield strength is 150MPa, the elongation is 30%, and after the pipe is sampled for bending, expansion and flattening tests, there are no cracks or orange peel phenomenon on the inner and outer surfaces.

[0062] Of course, for other types of aluminum alloys that can be strengthened by heat treatment, such as a specific type of 2XXX and 7XXX series aluminum alloys, thin-walled aluminum alloy pipes prepared using this preparation process can also refine the grains and improve the tensile strength and elongation.

[0063] It should be clear that the various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The present invention is not limited to the specific steps and structures described above and shown in the figures. In addition, for the sake of brevity, a detailed description of known methods and technologies is omitted here.

[0064] The above are only embodiments of the present application and are not limited to the present application. For those skilled in the art, the present application may have various changes and variations without departing from the scope of the present invention. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A process for preparing a heat-treatable and strengthened aluminum alloy thin-walled tube, characterized in that: The preparation process comprises the following steps: Step 1, extruding the heat-treatable and strengthened aluminum alloy ingot to obtain an extruded tube blank; Step 2, surface treating the extruded tube blank; Step 3, subjecting the surface treated extruded tube blank to multiple passes of high processing rate cold rolling to obtain a rolled tube blank; Step 4, pickling the rolled tube blank; Step 5, placing the pickled rolled tube billet vertically in a heat treatment furnace for intermediate solution annealing; Step 6, subjecting the tube blank after the intermediate solid solution annealing treatment to at least one pass of high processing rate cold rolling, and when the target finished tube is obtained, proceed to step 7; when the target finished tube is not obtained, loop through steps 4 to 6 until the target finished tube is obtained; Step 7, pickling the target finished pipe; Step 8, placing the target finished pipe after pickling treatment vertically in a heat treatment furnace for finished solution annealing to obtain a finished pipe; the finished pipe is 6061-T4 aluminum alloy; In step 5, the rolled tube is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-560° C., put into the furnace at the temperature, kept at the temperature for 20-60 minutes, and then water quenched; In step 3, the processing rate of each pass is 20-50%, and the total processing rate is 45-85%; in step 6, the processing rate of each pass is 20-55%, and the total processing rate is 55-95%.

2. The process for preparing the heat-treatable and strengthened aluminum alloy thin-walled pipe according to claim 1, characterized in that: In step 2, the inner and outer surfaces and end faces of the extruded tube are turned and the inner and outer surfaces are polished.

3. The process for preparing the heat-treatable and strengthened aluminum alloy thin-walled pipe according to claim 1, characterized in that: In step 8, the finished pipe is placed vertically in a heat treatment furnace at a heat treatment temperature of 520-580° C., put into the furnace when the temperature reaches the temperature, and kept at the temperature for 30-60 minutes before water quenching.

4. The process for preparing the heat-treatable and strengthened aluminum alloy thin-walled pipe according to claim 1, characterized in that: The outer diameter of the finished pipe is 6-120 mm, and the wall thickness is 0.5-2.5 mm.

5. The process for preparing the heat-treatable and strengthened aluminum alloy thin-walled tube according to any one of claims 1 to 4, characterized in that: The finished pipe is made of 6061-T4 aluminum alloy, with a tensile strength of 266-287 MPa, a yield strength of 135-165 MPa, and an elongation of 27.5-34.5%.