Proton exchange membrane electrolyzer membrane electrode with gradient pore catalytic layer and preparation method thereof

Through the design of gradient pore catalytic layer and ultrasonic spraying technology, the problems of pore structure and interface control in the existing membrane electrode catalytic layer design are solved, the performance and industrialization potential of membrane electrodes are improved, and efficient hydrogen energy preparation is achieved.

CN116053542BActive Publication Date: 2024-11-19NORTH CHINA ELECTRIC POWER UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310090270.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2024-11-19
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

The catalytic layer design of the existing proton exchange membrane electrolytic hydrogen-making membrane electrode lacks clear pore structure and interface control, resulting in poor performance of the membrane electrode, and the existing process is complex and difficult to industrialize on a large scale.

Method used

The preparation method of proton exchange membrane electrolytic cell membrane electrode with gradient pore catalytic layer was adopted. The Pt/C and IrO2 catalyst suspension was formed on both sides of the Nafion membrane by ultrasonic spraying technology, and the advantages of CCM and CCS technology were combined with the near-membrane. A high-load low-pore catalytic layer is formed on the side, and a low-load high-pore catalytic layer is formed on the side of the near-diffusion layer, optimizing the catalyst distribution and interface structure.

Benefits of technology

The catalytic reaction rate and performance of the membrane electrode are improved, the total load of precious metal catalysts is reduced, the preparation process is simplified, the production cost is reduced, and more efficient hydrogen energy preparation is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116053542B_ABST
    Figure CN116053542B_ABST
Patent Text Reader

Abstract

A proton exchange membrane electrolyzer membrane electrode with a gradient pore catalytic layer and a preparation method thereof, involving the preparation of a proton exchange membrane electrolyzer membrane electrode with a gradient laminated pore catalytic layer using platinum carbon and iridium oxide as catalyst coatings: a laminated catalytic structure with different pores is realized on the membrane side and near the diffusion layer side of the membrane electrode catalyst layer, and the performance of the membrane electrode is significantly improved by adjusting the ratio of precious metal nanoparticles and modified electrode perfluorosulfonic acid, and combining the advantages of catalyst coating membrane technology and catalyst coating diffusion layer technology, and presenting gradient pores and better surface wettability, which not only greatly improves the three-term interface reaction rate of the membrane electrode catalyst layer, but also is easy to operate and can continuously prepare large-area membrane electrode products. The design idea can also be used in the design of the catalytic layer of proton exchange membrane fuel cells, as well as in the fields of metal nanoparticles such as anion exchange membranes and catalysts deposited on both sides of the membrane to create three-term interfaces to accelerate reaction rates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of producing proton exchange membrane water electrolysis hydrogen production membrane electrodes by surface processing and coating methods and the field of catalytic material science, and particularly relates to a method for preparing a proton exchange membrane electrolyzer membrane electrode having a gradient laminated porous catalytic layer with platinum carbon and iridium oxide as catalyst coating. Background Art

[0002] Under the policy background of the "dual carbon" goal, renewable energy and intermittent power sources represented by fluctuating power sources such as wind and solar power have developed rapidly. Hydrogen energy is considered to be the best means to store energy from fluctuating power sources. Proton exchange membrane electrolysis of water to produce hydrogen is an important method of hydrogen production. With its rapid response and high energy density, it solves the energy storage problem of discontinuity of fluctuating power generation, while providing a sustainable solution for the efficient and clean production of hydrogen.

[0003] At present, the ultrasonic spraying preparation method of the membrane electrode with platinum carbon and iridium dioxide as the catalyst coating tends to be single and uniform in the design of the catalyst layer, and there is no clear guidance on the pore structure and interface control design of the catalyst layer. The prior art, such as the Chinese patent application, its application number: CN202210623065, publication number: CN114959765A, discloses a membrane electrode adhesive and a membrane electrode slurry preparation method, a membrane electrode and a proton exchange membrane water electrolysis cell. The membrane electrode slurry is prepared by adding nano-microspherical fluorocarbon polymer as an adhesive. The preparation process adds a lot of organic matter and the process is complicated. In addition, the slurry adds hydrophobic materials, which has a great influence on the wettability of the catalyst layer interface and thus affects the membrane electrode performance. Prior art, such as Chinese patent application, application number: CN201780021158, publication number: CN109075348A, discloses a method for manufacturing a membrane electrode assembly, a membrane electrode assembly manufactured thereby, and a fuel cell including the membrane electrode assembly. Glycerol and isopropanol are added to a dry catalyst slurry mixture, and the catalyst slurry composition is ultrasonically re-homogenized to improve the dispersion of the ionomer. However, this operation is not an absolute factor affecting the actual membrane surface deposition of the membrane electrode, and the slurry conditions of the control group are too absolute, resulting in precipitation of catalyst particles. Poor uniformity leads to differences in the final membrane electrode performance, and the application prospect is not high.

[0004] The prior art does not clearly propose a method for regulating the pore structure and interfacial wetting characteristics of the catalyst layer stack by regulating the membrane electrode slurry ratio and spraying parameters. In addition, the existing preparation methods of membrane electrodes for proton exchange membrane electrolyzers tend to prepare uniform catalyst slurry, which is only the experimental basis for preparing membrane electrodes and one of the parameters that affect the final performance of membrane electrodes. It has limitations, but the application of high-performance membrane electrodes prepared in the laboratory to large-scale industrialization still requires process parameter support. Therefore, clarifying a preparation method for membrane electrodes for proton exchange membrane electrolyzers with gradient pore catalytic layers is of great significance to the development of the technology of membrane electrode preparation for proton exchange membrane water electrolysis hydrogen production. Summary of the invention

[0005] The present invention uses anode IrO2, cathode Pt / C nanoparticles and Nafion as the main body of the catalyst layer, and discloses a method for preparing a membrane electrode of a proton exchange membrane electrolyzer with a gradient pore catalyst layer, comprising the following steps:

[0006] A method for preparing a membrane electrode for a proton exchange membrane electrolyzer having a gradient pore catalytic layer, characterized in that it comprises the following steps:

[0007] Step 1: 40% Pt / C and 5wt% Nafion solution are mixed according to the solid mass ratio, and ultrapure water and isopropanol are added in turn according to the volume ratio. After adding the ultrapure water, isopropanol is added again after ultrasonication in an ice-water bath, and the solid content of the prepared catalyst slurry is ensured to be 2wt%. Ultrasonication is performed in an ice-water bath again to uniformly mix the substances in the slurry. The ultrasonicated slurry is ultrasonically crushed in an ice-water bath for multiple times to disperse the catalyst particles in the solvent to form a cathode Pt / C catalyst suspension 1;

[0008] Step 2: 20% Pt / C is mixed with 5wt% Nafion solution in a solid mass ratio, IrO2 is mixed with 5wt% Nafion solution in a solid mass ratio, and IrO2 is mixed with 5wt% Nafion solution in a solid mass ratio, and the process in step 1 is repeated to form cathode Pt / C catalyst suspension 2, anode IrO2 catalyst suspension 3 and anode IrO2 catalyst suspension 4;

[0009] Step 3: Place all the prepared slurries under magnetic stirring and wait for use;

[0010] Step 4: Cut the Nafion115 membrane into blocks of a certain area, treat it in a 5wt% hydrogen peroxide solution and then rinse it with deionized water; treat it in a 1mol / L sulfuric acid solution and then rinse it with deionized water to activate the proton conductivity of the Nafion membrane, then put it into a blast drying oven to dry it for use, and obtain a pretreated proton exchange membrane;

[0011] Step 5: Place the treated Nafion115 membrane on the vacuum adsorption heating plate of the ultrasonic spraying equipment, maintain the temperature of the hot plate, ensure that the membrane surface is flat and covered with a quartz mask to determine the spraying center position, ensure the effective loading area of ​​the membrane electrode, set the nitrogen carrier gas pressure, slurry spraying flow rate, nozzle moving speed, and ultrasonically spray and deposit the Pt / C catalyst suspension 1 and IrO2 catalyst suspension 3 on both sides of the Nafion115 membrane to form a catalytic layer structure on both sides of the Nafion membrane;

[0012] Step 6: Separate the Toray H60 and titanium fiber felt, clean them with acetone, ethanol and deionized water respectively by ultrasonic, and then put them in a blast dryer for later use;

[0013] Step 7: Setting the nitrogen carrier gas pressure gauge pressure, slurry spraying flow rate, and nozzle moving speed, ultrasonically spraying the Pt / C catalyst suspension 2 and the IrO2 catalyst suspension 4 onto the cathode diffusion layer carbon paper and the anode diffusion layer titanium felt, respectively, to form a cathode catalyst layer 2 and an anode catalyst layer 4, and preparing a gas diffusion electrode for proton exchange membrane water electrolysis;

[0014] Step 8: Use PET film to heat-press and seal the membrane electrode prepared in step 6, heat-seal each side of the membrane electrode, place the anode and cathode gas diffusion electrodes in step 6 on both sides of the anode and cathode catalyst layers of the membrane electrode prepared in step 5, respectively, place them in a metal pressing plate and put them in a hot press, set the hot plate temperature, pressure, and holding time, and obtain a proton exchange membrane water electrolysis gradient pore structure membrane electrode.

[0015] The present invention also discloses a proton exchange membrane electrolyzer membrane electrode structure with a gradient pore catalytic layer, which is characterized in that the anode and cathode catalytic layers of the membrane electrode are divided into two layers, and a gradient distribution is formed near the membrane side and the diffusion layer side to ensure that the reaction occurs more efficiently.

[0016] The present invention also discloses a membrane electrode in a single cell testing system, which is used to measure the membrane electrode of a proton exchange membrane electrolyzer prepared by the method described in claim 2; the system is characterized in that: deionized water enters a water heater from a storage tank through a cross-flow peristaltic pump, and then reacts on the anode side of a single cell test fixture to generate oxygen, which is refluxed into the storage tank; a PID temperature controller controls a thermal resistor to heat the water heater and the membrane electrode test fixture body, and an electrochemical test characterization is performed on the membrane electrode through an electrochemical workstation; the anode adopts a titanium plate serpentine flow field, and the diffusion layer is a Freudenberg 0.25 mm thick titanium felt; the cathode adopts a graphite plate serpentine flow field, and the diffusion layer is a Toray H60 carbon paper, with an effective area of ​​2.5×2.5 cm2, the peristaltic pump deionized water flow rate is 20 ml / min, the electrolytic cell temperature is 80°C, and the polarization curve is tested by a GAMRY electrochemical workstation.

[0017] At present, commercial membrane electrodes on the market generally use one of the methods of catalyst coated membrane technology (CCM technology) or catalyst coated diffusion layer to prepare gas diffusion electrode (GDE) technology (CCS technology), but each has its advantages and disadvantages. The advantage of CCM technology is that the contact resistance between the catalyst layer and the membrane is small, but the membrane is easily swollen and damaged during the preparation process. CCS technology is easy to prepare, but the contact resistance is large. The catalyst slurry uses a specific proportion of Nafion content to form a uniform membrane electrode anode catalyst layer and cathode catalyst layer, that is, the anode catalyst layer is a Nafion content, and the cathode catalyst layer is a Nafion content. In practice, there are catalytic reactions of different rates inside the catalyst layer near the Nafion membrane end and the diffusion layer end of the membrane electrode, and the catalyst utilization rate of the catalyst layer near the membrane side is high.

[0018] 1. In the present invention, the respective advantages of CCM technology and CCS technology are combined with the intensity of the reaction near the membrane side and the near diffusion layer side of the catalyst layer and the demand for loading. A catalyst-coated membrane (CCM) structure with a catalyst layer with a high Nafion polymer content is formed on the Nafion membrane side by layered spraying, so as to achieve a catalyst layer bottom layer with high loading and low porosity near the membrane side. On the basis of this diffusion layer, a catalyst with a low Nafion polymer content is continuously sprayed to form a gas diffusion electrode (GDE), forming a catalyst layer upper layer with high porosity and low loading near the diffusion layer side. Thus, a stratified distribution of catalysts with a pore gradient is formed in the catalyst layer, which not only meets the advantages of high catalyst loading and high utilization rate of the catalyst layer near the membrane side, but also forms a high-pore interface near the diffusion layer side, which is conducive to gas-liquid two-phase transmission.

[0019] 2. The present invention improves the catalyst slurry suspension Nafion and spraying process to design the membrane electrode catalyst layer in layers, distributes the catalyst layer near the membrane side and near the diffusion layer side, and forms a layered structure with high loading and low pore size near the membrane side and low loading and high pore size near the diffusion layer side, which is beneficial to the distribution of three-phase water vapor flow at the interface and improves the gas-liquid two-phase transmission on the catalyst layer surface, thereby accelerating the catalytic reaction rate and improving the performance of the membrane electrode. The total loading of precious metals is reduced, the production and preparation costs are reduced, and the performance of the membrane electrode assembly is better.

[0020] 3. The membrane electrode catalyst layer stacking structure designed by the present invention can not only be used to prepare membrane electrodes for proton exchange membrane electrolyzers, but can also be used in the design of catalyst layers for proton exchange membrane fuel cells, as well as in the fields of anion exchange membranes and other fields where catalysts such as metal nanoparticles are deposited on both sides of the membrane to create three-way interfaces to accelerate reaction rates. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1The schematic diagram of the longitudinal section of the commercial membrane electrode and the membrane electrode prepared in Example 3. Its characteristic is that the cathode and anode catalyst layers of the membrane electrode are divided into two layers, and a gradient distribution is formed near the membrane side and the diffusion layer side to ensure that the reaction occurs more efficiently.

[0022] Figure 2 The flow chart of membrane electrode preparation of the present invention is as follows: The catalytic layer near the membrane side of the Nafion membrane is sprayed by an ultrasonic sprayer, and the diffusion layer is ultrasonically sprayed near the diffusion layer side to form the diffusion layer, and finally the diffusion layer is uniformly hot-pressed.

[0023] Figure 3 This is a schematic diagram of the membrane electrode experimental test system of the embodiment. Deionized water enters the water heater from the storage tank through the cross-flow peristaltic pump, and then reacts on the anode side of the single cell test fixture to generate oxygen, which flows back into the storage tank. The PID temperature controller controls the thermal resistor to heat the water heater and the membrane electrode test fixture body, and the membrane electrode is electrochemically tested and characterized by the Gamry electrochemical workstation.

[0024] Figure 4 Schematic diagram of the single battery fixture structure.

[0025] Figure 5 The polarization curves of the membrane electrodes of Examples 1, 2, and 3 were measured in a single cell test system under the test conditions of a cell temperature of 80° C. and a water inlet flow rate of 20 ml / min. Implementation

[0026] In order to make the test data comparable, polarization curve tests were performed on different membrane electrodes in the same single cell fixture and under the same test conditions, and the test conditions were unified as follows:

[0027] The anode uses a titanium plate serpentine flow field, and the diffusion layer is Freudenberg 0.25mm thick titanium felt; the cathode uses a graphite plate serpentine flow field, and the diffusion layer is Toray H60 carbon paper, with an effective area of ​​2.5×2.5cm 2 , the peristaltic pump deionized water flow rate is 20ml / min, the electrolytic cell temperature is 80℃, and the polarization curve is tested by GAMRY electrochemical workstation.

[0028] Embodiment 1:

[0029] Step 1: 40% Pt / C and 5wt% Nafion solution were mixed at a solid mass ratio of 4:1, and ultrapure water and isopropanol were added in a volume ratio of 1:10. After adding ultrapure water, isopropanol was added again after ultrasonication in an ice-water bath for 10 minutes, and the solid content of the prepared catalyst slurry was ensured to be 2wt%. The slurry was ultrasonicated in an ice-water bath for 10 minutes again to make the substances in the slurry evenly mixed. The ultrasonicated slurry was ultrasonically crushed for 3 consecutive times in an ice-water bath for 10 minutes to make the catalyst particles well dispersed in the solvent to form a cathode Pt / C catalyst suspension 1;

[0030] Step 2: Place all the prepared slurries under magnetic stirring at 900 rpm overnight for later use;

[0031] Step 3: Cut the Nafion115 membrane into several squares with an area of ​​4×4 cm2, treat it in a 5wt% hydrogen peroxide solution at 80°C for 60 minutes, rinse it with deionized water to remove surface impurities, treat it in a 1mol / L sulfuric acid solution at 80°C for 60 minutes, rinse it with deionized water again to remove surface metal impurities, activate the proton conductivity of the Nafion membrane, and then put it into a blast drying oven at 50°C for 1h and wait for use to obtain a pretreated proton exchange membrane;

[0032] Step 4: Place the treated Nafion115 membrane on the vacuum adsorption heating plate of the ultrasonic spraying equipment, maintain the temperature of the hot plate at 90°C, ensure that the membrane surface is flat and covered with a quartz mask to determine the center position of the spraying, ensure that the effective load area of ​​the membrane electrode is 2.5×2.5cm2, set the nitrogen carrier gas pressure gauge pressure to 100pa, the slurry spray flow rate to 1ml / min, and the nozzle moving speed to 15mm / s, and ultrasonically spray and deposit the Pt / C catalyst suspension 1 and the IrO2 catalyst suspension 3 on both sides of the Nafion115 membrane to form a catalytic layer structure on both sides of the Nafion membrane. (i.e. Figure 1 Middle 1- cathode catalyst layer-Naifon115-1- anode catalyst layer);

[0033] Step 5: Cut Toray H60 and titanium fiber felt into 2.6×2.6 cm2, ultrasonically clean them with acetone, ethanol and deionized water for 10 minutes respectively, put them into a forced air drying oven at 50°C for 1 hour and wait for use.

[0034] Step 6: Use PET film to heat-press and seal the membrane electrode prepared in step 4, heat-seal each side of the membrane electrode for 5 seconds, place the diffusion layer in step 5 on both sides of the anode and cathode catalyst layers of the membrane electrode prepared in step 5, place it in a metal pressing plate and put it into a hot press, set the hot plate temperature to 140°C, the pressure to 450kg, and the pressure holding time to 10 minutes to obtain a CCM membrane electrode. Example

[0035] Step 1: 20% Pt / C and 5wt% Nafion solution are mixed at a solid mass ratio of 8:1, IrO2 and 5wt% Nafion solution are mixed at a solid mass ratio of 10:1, and IrO2 and 5wt% Nafion solution are mixed at a solid mass ratio of 5:1-10:1, and the process in step 1 is repeated to form a cathode Pt / C catalyst suspension 2, an anode IrO2 catalyst suspension 3, and an anode IrO2 catalyst suspension 4;

[0036] Step 2: Place all the prepared slurries under magnetic stirring at 900 rpm overnight for later use;

[0037] Step 3: Cut the Nafion115 membrane into several squares with an area of ​​4×4 cm2, treat it in a 5wt% hydrogen peroxide solution at 80°C for 60 minutes, rinse it with deionized water to remove surface impurities, treat it in a 1mol / L sulfuric acid solution at 80°C for 60 minutes, rinse it with deionized water again to remove surface metal impurities, activate the proton conductivity of the Nafion membrane, and then put it into a blast drying oven at 50°C for 1h and wait for use to obtain a pretreated proton exchange membrane;

[0038] Step 4: Cut Toray H60 and titanium fiber felt into 2.6×2.6cm pieces 2 After ultrasonic cleaning with acetone, ethanol and deionized water for 10 minutes respectively, it was placed in a forced air drying oven at 50°C for 1 hour and waited for use.

[0039] Step 5: Set the nitrogen carrier gas pressure gauge to 100 Pa, the slurry spraying flow rate to 1.5 ml / min, and the nozzle moving speed to 20 mm / s, and ultrasonically spray the Pt / C catalyst suspension 2 and the IrO2 catalyst suspension 4 onto the cathode diffusion layer carbon paper and the anode diffusion layer titanium felt, respectively, to form Figure 1 The cathode catalyst layer 2 and the anode catalyst layer 4 are used to prepare a gas diffusion electrode for proton exchange membrane water electrolysis (i.e., anode diffusion layer-2-anode catalyst layer, cathode diffusion layer-2-cathode catalyst layer);

[0040] Step 6: Use PET film to heat-press and seal the Nafion115 prepared in step 3, and heat-seal each side of the membrane electrode for 5 seconds. Place the anode and cathode gas diffusion electrodes in step 5 on both sides of the Nafion membrane prepared in step 3, respectively, and put them in a metal pressing plate and put them into a hot press. Set the hot plate temperature to 140°C, the pressure to 450kg, and the pressure holding time to 10 minutes to obtain a gas diffusion electrode CCS type membrane electrode.

[0041] Embodiment 3:

[0042] Step 1: 40% Pt / C and 5wt% Nafion solution were mixed at a solid mass ratio of 4:1, and ultrapure water and isopropanol were added in a volume ratio of 1:10. After adding ultrapure water, isopropanol was added again after ultrasonication in an ice-water bath for 10 minutes, and the solid content of the prepared catalyst slurry was ensured to be 2wt%. The slurry was ultrasonicated in an ice-water bath for 10 minutes again to make the substances in the slurry evenly mixed. The ultrasonicated slurry was ultrasonically crushed for 3 consecutive times in an ice-water bath for 10 minutes to make the catalyst particles well dispersed in the solvent to form a cathode Pt / C catalyst suspension 1;

[0043] Step 2: 20% Pt / C is mixed with 5wt% Nafion solution at a solid mass ratio of 8:1, IrO2 is mixed with 5wt% Nafion solution at a solid mass ratio of 10:1, and IrO2 is mixed with 5wt% Nafion solution at a solid mass ratio of 5:1-10:1, and the process in step 1 is repeated to form cathode Pt / C catalyst suspension 2, anode IrO2 catalyst suspension 3 and anode IrO2 catalyst suspension 4;

[0044] Step 3: Place all the prepared slurries under magnetic stirring at 900 rpm overnight for standby use, and stir to keep the catalyst slurry uniform as a whole;

[0045] Step 4: Cut the Nafion115 membrane into several squares with an area of ​​4×4 cm2, treat it in a 5wt% hydrogen peroxide solution at 80°C for 60 minutes to remove impurities on the membrane surface, then rinse it with deionized water to remove surface impurities, then treat it in a 1mol / L sulfuric acid solution at 80°C for 60 minutes to remove surface metal ions, then rinse it with deionized water to activate the proton conductivity of the Nafion membrane, then put it in a blast drying oven at 50°C for 1 hour and wait for use, to obtain a pretreated proton exchange membrane;

[0046] Step 5: Place the treated Nafion 115 membrane on the vacuum adsorption heating plate of the ultrasonic spray equipment, maintain the temperature of the hot plate at 90°C, ensure that the membrane surface is flat and covered with a quartz mask to determine the center position of the spraying, and ensure that the effective loading area of ​​the membrane electrode is 2.5×2.5cm 2 , set the nitrogen carrier gas pressure gauge pressure to 100pa, the slurry spraying flow rate to 1ml / min, and the nozzle moving speed to 15mm / s. The carrier gas pressure is conducive to making the catalyst atomized droplets with the load more evenly dispersed. The spraying flow rate and moving speed match is conducive to the rapid evaporation of the isopropanol from the catalyst slurry sprayed on the membrane, leaving the catalyst loaded on the membrane. The Pt / C catalyst suspension 1 and the IrO2 catalyst suspension 3 are ultrasonically sprayed and deposited on both sides of the Nafion115 membrane to form a catalytic layer structure on both sides of the Nafion membrane. (i.e. Figure 11- cathode catalyst layer-Naifon115-1- anode catalyst layer);

[0047] Step 6: Cut Toray H60 and titanium fiber felt into 2.6×2.6cm pieces 2 After ultrasonic cleaning with acetone, ethanol and deionized water for 10 minutes respectively, it was placed in a forced air drying oven at 50°C for 1 hour and waited for use.

[0048] Step 7: Set the nitrogen carrier gas pressure gauge to 100 Pa, the slurry spraying flow rate to 1.5 ml / min, and the nozzle moving speed to 20 mm / s, and ultrasonically spray the Pt / C catalyst suspension 2 and the IrO2 catalyst suspension 4 onto the cathode diffusion layer carbon paper and the anode diffusion layer titanium felt, respectively, to form Figure 1 The cathode catalyst layer 2 and the anode catalyst layer 4 are used to prepare a gas diffusion electrode for proton exchange membrane water electrolysis (i.e., anode diffusion layer-2-anode catalyst layer, cathode diffusion layer-2-cathode catalyst layer);

[0049] Step 8: The membrane electrode prepared in step 6 is heat-pressed and sealed with PET film. Each side of the membrane electrode is heat-sealed for 5 seconds. The cathode and anode gas diffusion electrodes in step 6 are placed on both sides of the cathode and anode catalyst layers of the membrane electrode prepared in step 5, respectively. The cathode and anode gas diffusion electrodes are placed in a metal pressing plate and placed in a hot press. The hot plate temperature is set to 140°C, the pressure is 450kg, the pressure is maintained for 10 minutes, and the hot pressing is ensured. Figure 1 The five-layer structure membrane electrode shown can be in close contact, reduce contact resistance, and obtain a proton exchange membrane water electrolysis gradient pore structure membrane electrode. (i.e., the structure of anode diffusion layer-2-anode catalyst-1-anode catalyst layer-proton exchange membrane-1-cathode catalyst layer-2-cathode catalyst layer-cathode diffusion layer).

[0050] By comparing the polarization curves of membrane electrodes 1, 2, and 3 obtained in the above examples Figure 2 It can be seen that: Example 3 uses steps 7 and 8 to prepare the catalyst layer in a gradient layered manner, forming a structural feature of high loading and small pores near the membrane side, low loading and large pores near the diffusion layer side, and at the same current density, the battery voltage is lower, the power consumption is lower, and the electrochemical performance is better. Compared with the membrane electrode catalyst layer with a homogeneous pore structure, the membrane electrode with a gradient laminated pore structure exhibits better polarization performance. Example 3 is the best example. Example

[0051] like Figure 1 As shown, Figure 1The difference between the five-layer structure of anode diffusion layer-anode catalyst layer-proton exchange membrane-cathode catalyst layer-cathode diffusion layer of the traditional membrane electrode structure shown on the left is that in the present invention, according to the utilization of the catalyst at the three-phase interface of the catalyst layer in the actual reaction process, the anode catalyst layer and the cathode catalyst layer are subjected to a more refined gradient layering treatment, that is, a seven-layer structure of anode diffusion layer-2-anode catalyst layer-1-anode catalyst layer-proton exchange membrane-1-cathode catalyst layer-2-cathode catalyst layer-cathode diffusion layer. In the catalyst layers on both sides close to the proton exchange membrane, that is, 1-anode catalyst layer and 1-cathode catalyst layer, a catalyst layer with high catalyst content and high polymer content is used to directly spray the catalyst on the membrane, which can take advantage of the high utilization rate of catalysts on both sides near the membrane to improve the overall performance. In the two catalyst layers close to the diffusion layer, that is, 2-anode catalyst layer and 2-cathode catalyst layer, a catalyst layer with low polymer content and low catalyst load is used to spray the diffusion layer, and the material transmission characteristics of the three-phase interface near the diffusion layer side are used to create a catalyst layer with larger pores and lower catalyst load, thereby reducing the catalyst load. At the same time, it also combines the characteristics of direct spray membrane CCM technology and direct spray diffusion layer CCS technology, and finally hot press molding, forming a gradient distribution near the membrane side and near the diffusion layer side to ensure that the reaction occurs more efficiently. This will comprehensively reduce the catalyst loading of the catalytic layer and improve performance. Example

[0052] like Figure 2 As shown, the catalyst slurry passes through the slurry inlet and is broken up by the ultrasonic nozzle under the push of N2 carrier gas, and is dispersed into extremely fine catalyst slurry droplets and sprayed out. The sprayed carriers such as the proton exchange membrane / diffusion layer are adsorbed on them by the vacuum heating plate and heated evenly to ensure that the sprayed surface is flat and the isopropanol solvent inside the slurry evaporates quickly after the slurry is sprayed on the surface, ensuring that the formed catalytic layer is uniform and preventing the proton exchange membrane from swelling due to uneven adsorption of the solvent, which affects the uniformity and flatness of the catalytic layer. Example

[0053] A membrane electrode in a single cell test system, such as Figure 3 Its characteristics are as follows: deionized water enters the water heater from the storage tank through the cross-flow peristaltic pump, and then reacts on the anode side of the single cell test fixture to generate oxygen, which flows back into the storage tank. The water heater and the membrane electrode test fixture body are heated by the thermal resistor controlled by the PID temperature controller, and the membrane electrode is electrochemically tested and characterized by the Gamry electrochemical workstation. During the electrochemical test, the step constant current method is used to test the battery voltage corresponding to the single cell fixture at different current densities and then combine them into a polarization curve.

[0054] and a single cell test fixture, such as Figure 4As shown, it is composed of an end plate, a bipolar plate, a polytetrafluoroethylene gasket and a heat-sealing film. The prepared membrane electrode is heat-shrunk on both sides of the heat-sealing film, and the polytetrafluoroethylene gasket is used to adjust the height and seal it, then it is clamped into the titanium bipolar plate and fixed with bolts for membrane electrode performance testing in a battery test system.

[0055] The present invention proposes to adopt an ultrasonic spraying method, use precious metal nano IrO2 and Pt / C as cathode and anode catalyst layer catalysts respectively, prepare a spray slurry suspension highly dispersed and keep the nanometer scale by adjusting the ratio of precious metal nano particles and modified electrode perfluorosulfonic acid (Nafion), the ratio of solid content and dispersant isopropanol, and ultrasonic crushing time, and prepare a membrane electrode catalyst layer by controlling the heating base plate temperature, nozzle moving speed, liquid flow, carrier gas pressure, and spraying cycle during the spraying process, so that the performance of the membrane electrode is significantly improved, and gradient pores and better surface wettability are presented, which can not only greatly improve the three interface reaction rates of the membrane electrode catalyst layer, but also the preparation process is simple to operate, and large-area membrane electrode products can be continuously prepared.

[0056] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a proton exchange membrane electrolyzer membrane electrode with a gradient pore catalytic layer, wherein the structure of the proton exchange membrane electrolyzer membrane electrode is as follows: the anode and cathode catalytic layers between the proton exchange membrane and the anode and cathode diffusion layers are evenly divided into two layers, a bottom catalytic layer with high load and low porosity is formed near the membrane side, and an upper catalytic layer with high porosity and low load is formed near the diffusion layer side to meet the requirements of more efficient reaction. It is characterized in that The following steps are involved: Step 1: 40% Pt / C and 5wt% Nafion solution are mixed at a solid mass ratio of 4:1, and ultrapure water and isopropanol are added in a volume ratio of 1:

10. After adding ultrapure water, isopropanol is added again after ultrasonication in an ice-water bath, and the solid content of the prepared catalyst slurry is ensured to be 2wt%. Ultrasonication is performed in an ice-water bath again to uniformly mix the substances in the slurry. The ultrasonicated slurry is ultrasonically crushed in an ice-water bath for multiple times to disperse the catalyst particles in the solvent to form a cathode Pt / C catalyst suspension 1; Step 2: Mix 20% Pt / C and 5wt% Nafion solution at a solid mass ratio of 8:1, and add IrO 2 It was mixed with 5wt% Nafion solution at a solid mass ratio of 10:1 to form IrO 2 and 5wt% Nafion solution at a solid mass ratio of 5:1 to 10:1, and repeat the process in step 1 to form cathode Pt / C catalyst suspension 2 and anode IrO 2 Catalyst suspension 3 and anode IrO 2 Catalyst suspension 4; Step 3: Place all the prepared slurries under magnetic stirring and wait for use; Step 4: Cut the proton exchange membrane into blocks of a certain area, treat it in a 5wt% hydrogen peroxide solution and then rinse it with deionized water; treat it in a 1mol / L sulfuric acid solution and then rinse it with deionized water to activate the proton conductivity of the proton exchange membrane, then put it into a blast drying oven to dry it for standby use, and obtain a pretreated proton exchange membrane; Step 5: Place the treated proton exchange membrane on the vacuum adsorption heating plate of the ultrasonic spraying equipment, maintain the temperature of the hot plate, ensure that the membrane surface is flat, cover the quartz mask to determine the spray center position, ensure the effective loading area of ​​the membrane electrode, set the nitrogen carrier gas pressure, slurry spray flow rate, nozzle movement speed, and place the Pt / C catalyst suspension 1 and IrO 2 The catalyst suspension 3 is ultrasonically sprayed and deposited on both sides of the proton exchange membrane to form a catalyst layer structure coated on both sides of the proton exchange membrane; Step 6: Cut the cathode diffusion layer carbon paper Toray H60 and titanium fiber felt, clean them with acetone, ethanol and deionized water respectively by ultrasonic, and put them in air drying for later use; Step 7: Set the nitrogen carrier gas pressure, slurry spraying flow rate, nozzle moving speed, and the Pt / C catalyst suspension 2 and IrO 2 The catalyst suspension 4 is ultrasonically sprayed on the cathode diffusion layer carbon paper Toray H60 and the titanium fiber felt to form a cathode catalyst layer 2 and an anode catalyst layer 4, respectively, to prepare anode and cathode gas diffusion electrodes; Step 8: The anode and cathode gas diffusion electrodes prepared in step 7 are heat-pressed and sealed with PET film. Each side of the anode and cathode gas diffusion electrodes is heat-sealed. The anode and cathode gas diffusion electrodes are respectively placed on both sides of the catalyst layer prepared in step 5. The electrodes are placed in a metal pressing plate and put into a hot press. The temperature, pressure and holding time of the hot plate are set to obtain a proton exchange membrane water electrolysis gradient pore structure membrane electrode.

2. A method for preparing a proton exchange membrane electrolyzer membrane electrode having a gradient pore catalytic layer according to claim 1, It is characterized in that The step 1 further includes the following contents: adding ultrapure water and isopropanol in a volume ratio of 1:10, adding the ultrapure water, ultrasonicating in an ice-water bath for 10 minutes, adding isopropanol again, and ensuring that the solid content of the prepared catalyst slurry is 2wt%, ultrasonicating in an ice-water bath for 10 minutes again to uniformly mix the substances in the slurry, and ultrasonically crushing the ultrasonicated slurry for 3 consecutive times for 10 minutes in an ice-water bath to ensure that the catalyst particles are well dispersed in the solvent.

3. The method for preparing a proton exchange membrane electrolyzer membrane electrode having a gradient pore catalytic layer according to claim 1, It is characterized in that The step 4 further comprises the following steps: cutting the proton exchange membrane into several pieces with an area of ​​4×4 cm 2 The cubes of different sizes were treated in a 5wt% hydrogen peroxide solution at 80℃ for 60 minutes, then rinsed with deionized water to remove surface impurities, and then treated in a 1mol / L sulfuric acid solution at 80℃ for 60 minutes, then rinsed with deionized water to remove surface metal impurities and activate the proton conductivity of the proton exchange membrane, and then placed in a forced air drying oven at 50℃ for 1h for use.

4. The method for preparing a proton exchange membrane electrolyzer membrane electrode having a gradient pore catalytic layer according to claim 1, It is characterized in that The step 5 further includes the following contents: placing the treated proton exchange membrane on the vacuum adsorption heating plate of the ultrasonic spraying equipment, maintaining the temperature of the hot plate at 90°C, ensuring that the membrane surface is flat and covered with a quartz mask to determine the spraying center position, and ensuring that the membrane electrode effective load area is 2.5×2.5 cm 2 , set the nitrogen carrier gas pressure gauge pressure to 100pa, the slurry spraying flow rate to 1ml / min, and the nozzle moving speed to 15mm / s.

5. The method for preparing a proton exchange membrane electrolyzer membrane electrode having a gradient pore catalytic layer according to claim 1, It is characterized in that The step 8 further includes the following contents: hot pressing and sealing the anode and cathode gas diffusion electrodes prepared in step 7 with PET film, and hot sealing each side of the anode and cathode gas diffusion electrodes for 5 seconds, placing the anode and cathode gas diffusion electrodes in step 7 on both sides of the catalyst layer prepared in step 5, respectively, placing them in a metal pressing plate and putting them into a hot press, setting the hot plate temperature to 140°C, the pressure to 450kg, and the holding time to 10 minutes to obtain a proton exchange membrane water electrolysis gradient pore structure membrane electrode.

6. A membrane electrode in a single cell testing system, the system being used to measure the membrane electrode of a proton exchange membrane electrolyzer prepared by the method of claim 1; Its characteristics are: Deionized water enters the water heater from the storage tank through a constant current peristaltic pump, and then reacts on the anode side of the single cell test fixture to generate oxygen, which flows back into the storage tank. The water heater and the membrane electrode test fixture body are heated by the thermal resistor controlled by the PID temperature controller, and the membrane electrode is electrochemically tested and characterized by the electrochemical workstation; the anode uses a titanium plate serpentine flow field and the diffusion layer is Freudenberg 0.25mm thick titanium fiber felt; the cathode uses a graphite plate serpentine flow field, and the cathode diffusion layer is carbon paper TorayH60, with an effective area of ​​2.5×2.5cm 2 , the peristaltic pump deionized water flow rate is 20ml / min, the electrolytic cell temperature is 80℃, and the polarization curve is tested by GAMRY electrochemical workstation.