Hydrodesulfurization catalyst suitable for low pressure conditions and preparation method and application thereof
By introducing specific elements and compounds into the hydrodesulfurization catalyst, a catalyst with high activity and stability under low pressure conditions is prepared, which solves the problem of poor catalyst stability in the existing technology, reduces hydrogen consumption, and improves clean diesel production. efficiency.
Patent Information
- Application Number
- CN202111273788.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing hydrodesulfurization catalysts have poor stability under low-pressure conditions and cannot effectively reduce hydrogen consumption during the diesel hydrogenation reaction, affecting the production of clean diesel.
A catalyst containing Group VIII metal elements, Group VIB metal elements, phosphorus elements, alumina carriers and organic alcohol compounds/carboxylic acid compounds is used, prepared by an impregnation method to control the composition and structure of the catalyst to improve its performance under low pressure conditions activity and stability.
A hydrodesulfurization catalyst with high activity and stability under low pressure conditions is provided, which reduces hydrogen consumption, improves the efficiency of clean diesel production, and has good industrial application value.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a hydrodesulfurization catalyst suitable for low-pressure conditions and a preparation method and application thereof. Background Art
[0002] With the continuous increase of social environmental awareness, the quality standards of fuel are gradually improving, and clean diesel production technology has attracted much attention from refineries. The use of advanced hydrodesulfurization catalysts is an economical and effective means to upgrade diesel quality. In the process of diesel hydrogenation, a large amount of hydrogen is required for hydrodesulfurization and aromatic saturation reactions. Under the trend of reducing carbon emissions, reducing the consumption of hydrogen in the diesel hydrogenation reaction process has become an important technical development direction. Generally, the operating pressure of the diesel hydrogenation reaction unit is relatively high, generally at 5-8MPa, which is easy to carry out aromatic saturation reaction, resulting in increased hydrogen consumption. Therefore, reducing the operating pressure of the unit is extremely important for reducing the hydrogen consumption of the reaction. However, most of the diesel hydrodesulfurization catalysts disclosed in existing patent applications are suitable for higher reaction pressure conditions, such as patent applications with application numbers 201711023399.5 and 201110045663.1. Therefore, it is necessary to develop a diesel hydrodesulfurization catalyst suitable for low-pressure conditions.
[0003] In view of the deficiencies of the prior art, the present invention prepares a hydrodesulfurization catalyst with superior performance suitable for low-pressure reaction conditions, which has high activity and stability and can meet the needs of clean diesel production. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem of poor stability of hydrodesulfurization catalysts under low-pressure conditions in the prior art, and to provide a hydrodesulfurization catalyst suitable for low-pressure conditions and a preparation method and application thereof. The catalyst has excellent stability and is particularly suitable for hydrodesulfurization reactions under low-pressure conditions, and can meet the needs of clean diesel production.
[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a hydrodesulfurization catalyst suitable for low-pressure conditions, which comprises at least one metal element of Group VIII, at least one metal element of Group VIB, phosphorus, an alumina carrier and at least one organic alcohol compound and / or a carboxylic acid compound; wherein the phosphorus content in the catalyst is 2-10 wt% as calculated on the basis of P2O5; wherein, based on the total amount of the catalyst, the content of the metal element of Group VIB is 12-28 wt% as calculated on the basis of the oxide; wherein, as calculated on the basis of the element, the atomic ratio of the cobalt element in the metal element of Group VIII to the total amount of the metal element of Group VIII is not less than 0.8.
[0006] Preferably, the alumina carrier contains phosphorus.
[0007] The second aspect of the present invention provides a method for preparing the hydrodesulfurization catalyst suitable for low-pressure conditions described in the first aspect, the method comprising: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and an organic alcohol compound and / or a carboxylic acid compound into an alumina carrier by an impregnation method, and then drying.
[0008] The third aspect of the present invention provides the use of the hydrodesulfurization catalyst suitable for low pressure conditions described in the first aspect in the hydrorefining of distillate oil.
[0009] The inventors found in their research that under low reaction pressure, hydrogen in the reaction system is relatively insufficient. In order to make the hydrodesulfurization reaction proceed smoothly, a hydrodesulfurization catalyst with high activity and stability is usually required. In the present invention, the composition of the hydrodesulfurization catalyst is regulated by introducing phosphorus and controlling the proportion of cobalt in the total amount of group VIII metal elements to provide a hydrodesulfurization catalyst with high activity and stability suitable for low pressure conditions.
[0010] In the present invention, on the one hand, phosphorus is introduced into the catalyst to reduce the alkaline center of the alumina carrier and increase the acidic center, weaken the interaction between the alumina carrier and the metal, and promote the dispersion of the active metal components. Preferably, part of the phosphorus element is introduced into the alumina carrier to further enhance the loading effect of the active metal components on the alumina carrier and enhance the dispersion of the active metal components. At the same time, organic alcohol compounds and / or carboxylic acid compounds are introduced into the catalyst to weaken the interaction between the carrier and the active center. In the presence of phosphorus on the surface of the alumina carrier, the role of organic alcohol compounds and / or carboxylic acid compounds is better exerted, so that the organic alcohol compounds and / or carboxylic acid compounds better promote the dispersion of active components, enhance the hydrodesulfurization effect of the catalyst under low pressure, improve the reaction efficiency for the clean production of diesel, and have excellent industrial value.
[0011] At the same time, the preparation process of the hydrodesulfurization catalyst has low requirements on production equipment, low production cost and good practical value. DETAILED DESCRIPTION
[0012] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0013] The first aspect of the present invention provides a hydrodesulfurization catalyst suitable for low-pressure conditions, the catalyst comprising at least one Group VIII metal element, at least one Group VIB metal element, phosphorus, an alumina carrier and at least one organic alcohol compound and / or a carboxylic acid compound; wherein, calculated as P2O5, the phosphorus content in the catalyst is 2-10 wt. %; wherein, based on the total amount of the catalyst, calculated as oxide, the content of the Group VIB metal element is 12-28 wt. %; wherein, calculated as an element, the atomic ratio of cobalt in the Group VIII metal element to the total amount of the Group VIII metal element is not less than 0.8.
[0014] The present invention provides a hydrodesulfurization catalyst suitable for low-pressure conditions containing the above-mentioned specific composition. The hydrodesulfurization catalyst still has good activity and stability under low-pressure conditions and is particularly suitable for hydrodesulfurization reactions under low-pressure conditions.
[0015] In the present invention, preferably, the metal element of Group VIII is cobalt and optionally one of other elements in Group VIII. In a preferred case, other elements in Group VIII include but are not limited to at least one of iron, nickel and palladium, preferably nickel.
[0016] In the present invention, there is no specific limitation on the selection range of the metal element of Group VIB. Preferably, the metal element of Group VIB includes but is not limited to at least one of chromium, molybdenum and tungsten, preferably molybdenum and / or tungsten.
[0017] In the present invention, there is no specific restriction on the amount of the metal element of Group VIII, as long as the performance of the hydrodesulfurization catalyst can be met. The amount of the active metal component in the hydrodesulfurization catalyst cannot be too much. Too much active metal component will reduce the desulfurization activity of the catalyst and reduce the stability of the catalyst. In a preferred case, the atomic ratio of cobalt element in the metal element of Group VIII to the total amount of metal elements of Group VIII is 0.85-1. The advantage of adopting this preferred embodiment is that when the content of cobalt element is within the above range, the hydrodesulfurization catalyst shows higher activity and stability under low pressure conditions, which is conducive to the long-term operation of the catalyst.
[0018] In a preferred embodiment, the atomic ratio of the metal element of group VIII to the total amount of the metal element of group VIII and the metal element of group VIB is 0.1-0.35: 1, preferably 0.2-0.3: 1. The advantage of adopting this preferred embodiment is to ensure good synergy between the metal element of group VIII and the metal element of group VIB, thereby improving the activity of the catalyst, so that the catalyst maintains good stability under low pressure conditions, and ensures long-term operation.
[0019] In the present invention, there is no specific restriction on the phosphorus content in the catalyst. Preferably, the phosphorus content in the catalyst is 3-10% by weight, more preferably 4-8% by weight, calculated as P2O5. The use of this preferred embodiment can further promote the dispersion of active metal components and better play the role of active components. The introduction of phosphorus can also enhance the acidic function of the catalyst and further improve the reaction effect of the catalyst under low pressure.
[0020] In the present invention, preferably, the phosphorus element in the catalyst comprises two parts. Preferably, the alumina carrier contains phosphorus element, hereinafter referred to as phosphorus-containing alumina. The advantage of adopting this preferred embodiment is that the alumina carrier contains a specific amount of phosphorus element, which can significantly promote the activity of the catalyst under low pressure conditions.
[0021] In a preferred embodiment, the phosphorus in the alumina carrier accounts for 10-40% by weight, preferably 10-35% by weight, of the total phosphorus content in the catalyst, calculated as P2O5. The advantage of adopting this preferred embodiment is to further improve the loading effect of the active metal component on the alumina carrier and improve the dispersion of the active metal component.
[0022] In the present invention, phosphorus can be introduced into the alumina carrier after molding, can be introduced during the molding process of the alumina carrier, and can also be introduced during the preparation process of the alumina carrier precursor. It is preferably introduced during the preparation process of the alumina carrier precursor. When introduced during the preparation process of the alumina precursor, phosphorus can be introduced by adding a phosphorus-containing compound during the preparation of the alumina precursor using the aluminum sulfate-sodium aluminate method. Specifically, phosphoric acid or phosphate is introduced as a raw material or introduced at any step in the preparation process of the alumina precursor. By introducing phosphorus into the alumina precursor, the structural properties of the alumina carrier are improved, and the dispersion ability of the active metal components is promoted.
[0023] In the present invention, the phosphorus element in the phosphorus-containing alumina carrier is provided by an alumina carrier precursor. In a preferred embodiment, the precursor of the alumina carrier is pseudo-boehmite, and the pseudo-boehmite contains phosphorus element.
[0024] Generally, a sodium-containing precursor (such as sodium oxide) is used when preparing pseudo-boehmite, and such substances will remain in the pseudo-boehmite. In a preferred embodiment, the sodium oxide content in the pseudo-boehmite does not exceed 0.08% by weight, preferably does not exceed 0.06% by weight. The advantage of adopting this preferred embodiment is to reasonably control the content of sodium oxide in the pseudo-boehmite, further reduce the basic center, make the catalyst have good activity and stability, and promote the hydrodesulfurization effect of the catalyst.
[0025] In the present invention, there is no specific limitation on the preparation method of the phosphorus-containing alumina carrier, and conventional preparation methods in the art are applicable to the present invention. Preferably, the phosphorus-containing alumina carrier is prepared by extrusion molding, and the specific operation method is not described in detail here.
[0026] In the present invention, in order to further improve the performance of the catalyst, a carrier with a specific composition and structure is selected as the carrier of the hydrodesulfurization catalyst. Preferably, the water absorption rate of the alumina carrier is greater than 0.9 mL / g, more preferably 1-1.1 mL / g, and the specific surface area is greater than 260 m 2 / g, more preferably 260-350m 2 / g, and the average pore size is greater than 10nm, more preferably 10-18nm.
[0027] In a preferred embodiment, in the alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina carrier, preferably no more than 8%, and more preferably 5-8%.
[0028] In a preferred embodiment, in the alumina carrier, the volume of pores with a pore size distribution of 2-4 nm accounts for no more than 4%, preferably no more than 2% of the total pore volume of the alumina carrier.
[0029] The use of the above-mentioned preferred alumina carrier with specific composition and structure can ensure that the catalyst has a relatively smooth pore structure, promote the diffusion of reaction molecules to the active center under low pressure, and thus improve the activity and stability of the catalyst.
[0030] In the present invention, the specific surface area, pore volume, pore diameter and pore distribution of the carrier are measured by low temperature nitrogen adsorption method (BET) (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). Among them, the pore volume of 2-100 nm is calculated according to the results of BET.
[0031] In the present invention, there is no specific restriction on the amount of the organic alcohol compound and / or the carboxylic acid compound, as long as it can meet the performance requirements of the hydrodesulfurization catalyst. Preferably, the molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the metal element of Group VIII is 0.5-6:1, preferably 1-5:1. The advantage of adopting this preferred embodiment is that the organic alcohol compound and / or the carboxylic acid compound can improve the dispersion of the active metal component, thereby improving the initial activity and stability of the hydrodesulfurization catalyst.
[0032] In the present invention, the type of organic alcohol compound is widely selected, and conventional organic alcohol compounds in the art are applicable to the present invention. Preferably, the organic alcohol compound can be at least one of a monohydric alcohol, a dihydric alcohol and a polyhydric alcohol. Further preferably, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane, and further preferably at least one of glycerol, propanol and ethylene glycol.
[0033] In the present invention, there is no specific limitation on the type of carboxylic acid compound. Preferably, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, and more preferably at least one of formic acid, citric acid and acetic acid.
[0034] In the present invention, there is no specific limitation on the size of the catalyst. Preferably, the equivalent diameter of the catalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm.
[0035] In the present invention, there is no specific limitation on the shape of the catalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the catalyst is cylindrical, clover, four-leaf clover, disc-shaped honeycomb or other irregular shapes, more preferably butterfly-shaped.
[0036] The second aspect of the present invention provides a method for preparing the hydrodesulfurization catalyst suitable for low-pressure conditions described in the first aspect, the method comprising: introducing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and an organic alcohol compound and / or a carboxylic acid compound into an alumina carrier by an impregnation method, and then drying.
[0037] In the present invention, the types of Group VIII metals, Group VIB metals, and organic alcohol compounds and / or carboxylic acid compounds have been described in the first aspect and will not be described in detail here.
[0038] In a preferred embodiment, the VIB Group metal precursor preferably includes but is not limited to one or more of ammonium heptamolybdate, ammonium molybdate, ammonium phosphomolybdate, molybdenum oxide, ammonium metatungstate, ethylammonium metatungstate and tungsten oxide.
[0039] In a preferred embodiment, the Group VIII metal precursor includes, but is not limited to, one or more of cobalt nitrate, basic cobalt carbonate, cobalt acetate, cobalt oxide, nickel nitrate, basic nickel carbonate, nickel acetate and nickel oxide.
[0040] In a preferred embodiment, the phosphorus-containing compound includes, but is not limited to, one or more of phosphoric acid, hypophosphorous acid, ammonium phosphate and diammonium phosphate.
[0041] According to the present invention, there is no specific limitation on the impregnation method, and conventional impregnation methods in the art are applicable to the present invention. For example, it can be one of co-impregnation, step-by-step impregnation, saturated impregnation and supersaturated impregnation. In a preferred embodiment, the present invention adopts a co-impregnation method to prepare a hydrodesulfurization catalyst suitable for low-pressure conditions. In a more preferred embodiment, the impregnation method comprises: impregnating the alumina carrier with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and an organic alcohol compound and / or a carboxylic acid compound.
[0042] In the present invention, there is no specific limitation on the order of adding the Group VIII metal precursor, the Group VIB metal precursor, the phosphorus-containing compound, and the organic alcohol compound and / or the carboxylic acid compound, as long as it is conducive to uniform mixing of the components. In a preferred embodiment, the organic alcohol compound and / or the carboxylic acid compound, the Group VIII metal precursor, and the Group VIB metal precursor are respectively added to an aqueous solution of the phosphorus-containing compound to provide the impregnation solution. In the present invention, the order of adding the organic alcohol compound and / or the carboxylic acid compound, the phosphorus-containing compound, and the metal precursor can also be interchanged.
[0043] In the present invention, the following preparation method can be specifically used to prepare the hydrodesulfurization catalyst: first dissolve the phosphorus-containing compound in water to obtain a phosphorus-containing aqueous solution, then add an organic alcohol compound and / or a carboxylic acid compound, a VIB group metal precursor and a VIII group metal precursor, stir under heating until completely dissolved, and keep the temperature constant to obtain an impregnation solution, measure the water absorption rate of the alumina carrier, and calculate the liquid absorption rate of the alumina carrier according to the formula of water absorption rate of the alumina carrier-0.1; according to the liquid absorption rate of the alumina carrier, the impregnation solution is fixed to a corresponding volume (alumina carrier liquid absorption rate×carrier mass), and the impregnation solution and the corresponding mass of the alumina carrier are evenly mixed and allowed to stand, and then dried to prepare a hydrodesulfurization catalyst suitable for low-pressure conditions.
[0044] In the present invention, the drying conditions have a wide range of selections. Preferably, the drying conditions include: a temperature of 80-200° C. and a time of 1-10 h.
[0045] The third aspect of the present invention provides use of the hydrogenation catalyst suitable for low pressure conditions described in the first aspect in the hydrorefining of distillate oil.
[0046] In a preferred embodiment, the sulfur content in the distillate to be treated does not exceed 13000 ppm, preferably 3000-13000 ppm.
[0047] In a preferred case, the catalyst needs to be vulcanized to convert the oxidized catalyst into a sulfurized catalyst before use. In the present invention, there is no specific limitation on the vulcanization method, and conventional vulcanization methods in the art are applicable to the present invention. Preferably, for example, it can be one of dry vulcanization and wet vulcanization. There is no particular limitation on the type of vulcanizing agent, and it can be selected according to conventional schemes in the art.
[0048] Preferably, the vulcanization conditions include: vulcanization temperature of 280-420°C, time of 10-48h, pressure of 0.1-15MPa, volume space velocity of 0.5-20h -1 , the volume ratio of hydrogen to oil is 100-2000:1, and the preferred heating rate is 5-60°C / hour.
[0049] In a preferred embodiment, the catalyst is used at a temperature of 320-400°C, a reaction pressure of 2-4.5 MPa, and a volume space velocity of 0.5-3 hours. -1 , the volume ratio of hydrogen to oil is 100-500:1.
[0050] The present invention will be described in detail below through examples. In the following examples, the hydrodesulfurization performance of the hydrodesulfurization catalyst suitable for low pressure conditions is measured on a small high pressure reaction device. First, the oxidized catalyst is converted into a sulfurized catalyst by a programmed temperature sulfurization method. The sulfurization conditions are: the sulfurization pressure is 6.4 MPa, the sulfurized oil is kerosene containing 22% by weight of CS, and the volume space velocity is 2 hours. -1 , the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then heat it up to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test, the reaction raw materials are diesel raw materials with a sulfur content of 9870ppm. The test conditions are: pressure of 4.0MPa, volume space velocity of 1.5h -1 , the hydrogen-oil volume ratio was 300 v / v, and the reaction temperature was 360°C. The product properties were analyzed after the reaction was stable for 2 days. In order to investigate the stability of the catalyst, the mass fraction of sulfur in the reaction product was kept at 10 ppm, the reaction temperature was adjusted every day, and the operation was continued for 5 days. The catalyst reaction temperature difference was used to represent the catalyst stability. The lower the temperature increase value, the better the catalyst stability.
[0051] The composition of the catalyst is calculated based on the feed amount. The specific surface area, pore distribution, pore volume and pore size of 2-100 nm pores in the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0052] Example 1
[0053] A certain amount of MoO3, basic cobalt carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0054] The carrier used to prepare the catalyst is a phosphorus-containing alumina carrier. The introduction of phosphorus into the carrier is obtained by adding a certain amount of phosphoric acid to the alumina for modification and calcining at 600°C for 3h. The water absorption rate of the phosphorus-containing alumina carrier is 1.08mL / g, and the specific surface area is 275m 2 / g, the average pore size is 12.2nm, the pore volume with a pore size of 2-6nm accounts for 5.2% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm. In addition, the sodium oxide content in the carrier is 0.05% by weight.
[0055] The prepared catalyst has a MoO3 content of 20% by weight, a Co / (Co+Mo) atomic ratio of 0.25, and a P2O5 content of 6% by weight, of which 30% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to the Group VIII metal is 1:1. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 7.8 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 1.7°C after 5 days of reaction.
[0056] Example 2
[0057] A certain amount of MoO3, basic cobalt carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0058] The carrier used to prepare the catalyst is a phosphorus-containing alumina carrier. The introduction of phosphorus into the carrier is obtained by adding a certain amount of phosphoric acid to the alumina for modification and calcining at 600°C for 3 hours. The water absorption rate of the phosphorus-containing alumina carrier is 1.05 mL / g, and the specific surface area is 269 m 2 / g, the average pore size is 11.9nm, the pore volume of pores with a pore size of 2-6nm accounts for 6.7% of the total pore volume, the pore volume of pores with a pore size of 2-4nm accounts for 1.9% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm. The sodium oxide content in the carrier is 0.03% by weight.
[0059] The prepared catalyst has a MoO3 content of 15% by weight, a Co / (Co+Mo) atomic ratio of 0.3, and a P2O5 content of 8% by weight, of which 20% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to the Group VIII metal is 2.5:1. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 9.8 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 1.8°C after 5 days of reaction.
[0060] Example 3
[0061] A certain amount of MoO3, basic cobalt carbonate, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0062] The carrier used to prepare the catalyst is a phosphorus-containing alumina carrier. The phosphorus element in the carrier is introduced by adding phosphoric acid during the preparation of the precursor pseudo-boehmite to obtain the phosphorus-containing alumina carrier. The phosphorus-containing alumina carrier is obtained after calcination at 600°C for 3 hours. The water absorption rate of the phosphorus-containing alumina carrier is 1.02mL / g, and the specific surface area is 286m 2 / g, the average pore size is 11.2nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm. The sodium oxide content in the carrier is 0.06% by weight.
[0063] In the prepared catalyst, the content of MoO3 is 22% by weight, the atomic ratio of (Co+Ni) / (Co+Ni+Mo) is 0.3, the atomic ratio of Co / (Co+Ni) is 0.8, and the content of P2O5 is 5% by weight, of which 25% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to the metal of Group VIII is 1.5:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 9.0ppm. When the sulfur content of the product is kept at 10ppm, the reaction temperature increases by 1.7°C after 5 days of reaction.
[0064] Example 4
[0065] A certain amount of MoO3, basic cobalt carbonate, basic nickel carbonate, and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0066] The carrier used to prepare the catalyst is the phosphorus-containing alumina carrier prepared in Example 3.
[0067] The prepared catalyst has a MoO3 content of 25% by weight, an atomic ratio of (Co+Ni) / (Co+Ni+Mo) of 0.27, an atomic ratio of Co / (Co+Ni) of 0.95, and a P2O5 content of 4% by weight, of which 10% by weight of P2O5 comes from the carrier. The molar ratio of citric acid to Group VIII metal is 1:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 6.9 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 1.8°C after 5 days of reaction.
[0068] Example 5
[0069] A certain amount of MoO3, basic cobalt carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 4 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0070] The carrier used to prepare the catalyst is the phosphorus-containing alumina carrier in Example 3.
[0071] The prepared catalyst has a MoO3 content of 18% by weight, a Co / (Co+Mo) atomic ratio of 0.3, a P2O5 content of 9% by weight, of which 35% by weight of P2O5 comes from the carrier. The molar ratio of citric acid to the Group VIII metal is 1:1. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 8.9 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 1.9°C after 5 days of reaction.
[0072] Example 6
[0073] A certain amount of ammonium metatungstate, basic cobalt carbonate, basic nickel carbonate, and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0074] The phosphorus-containing alumina carrier in Example 3 was used to prepare the catalyst carrier.
[0075] The prepared catalyst has a WO3 content of 25% by weight, an atomic ratio of (Co+Ni) / (Co+Ni+W) of 0.3, an atomic ratio of Co / (Co+Ni) of 0.95, and a P2O5 content of 9% by weight, of which 15% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to Group VIII metal is 1.5:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 7.0 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 2.0°C after 5 days of reaction.
[0076] Example 7
[0077] The catalyst was prepared according to the method of Example 2, except that the sodium oxide in the carrier alumina was 0.13 wt%. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 15.5 ppm. When the sulfur content of the product was kept at 10 ppm, the reaction temperature increased by 1.9° C. after 5 days of reaction.
[0078] Example 8
[0079] A certain amount of MoO3, basic cobalt carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0080] The carrier used to prepare the catalyst is a γ-alumina carrier with a water absorption rate of 1.04 mL / g and a specific surface area of 270 m 2 / g, the average pore size is 11.8nm, the pore volume of pores with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume of pores with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm. The sodium oxide content in the carrier is 0.13% by weight.
[0081] The prepared catalyst has a MoO3 content of 20% by weight, a Co / (Co+Mo) atomic ratio of 0.28, a P2O5 content of 6% by weight, and no phosphorus in the carrier. The molar ratio of propylene glycol to the Group VIII metal is 5:1. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 18.0 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 2.3°C after 5 days of reaction.
[0082] Example 9
[0083] A certain amount of MoO3, basic cobalt carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0084] The carrier used to prepare the catalyst is a phosphorus-containing alumina carrier. The pseudo-boehmite precursor used in the carrier preparation contains phosphorus, and phosphoric acid is added as a raw material during the preparation of the pseudo-boehmite precursor. The water absorption rate of the prepared phosphorus-containing alumina carrier is 1.03 mL / g, and the specific surface area is 285 m 2 / g, the average pore size is 11.8nm, the pore volume of pores with a pore size of 2-6nm accounts for 6.5% of the total pore volume, the pore volume of pores with a pore size of 2-4nm accounts for 1.2% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm. In addition, the sodium oxide content in the carrier is 0.05% by weight.
[0085] The prepared catalyst has a MoO3 content of 20% by weight, a Co / (Co+Mo) atomic ratio of 0.25, and a P2O5 content of 6% by weight, of which 30% by weight of the P2O5 comes from the carrier. The molar ratio of propylene glycol to the Group VIII metal is 1:1. After the catalyst is sulfurized and tested for reaction, the sulfur content in the product is 6.8 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 1.5°C after 5 days of reaction.
[0086] Comparative Example 1
[0087] A certain amount of MoO3, basic cobalt carbonate, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape. Comparative Example 1 The phosphorus-containing alumina carrier in Example 1 was selected.
[0088] The prepared catalyst has a MoO3 content of 32% by weight, an atomic ratio of (Co+Ni) / (Co+Ni+Mo) of 0.18, an atomic ratio of Co / (Co+Ni) of 0.85, and a P2O5 content of 6% by weight, of which 8% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to the metal element of Group VIII is 1:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 32.0 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature rises by 3.3°C after 5 days of reaction.
[0089] Comparative Example 2
[0090] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape. Comparative Example 2 selected the phosphorus-containing alumina carrier in Example 1.
[0091] The prepared catalyst has a MoO3 content of 20% by weight, an atomic ratio of Ni / (Ni+Mo) of 0.25, and a P2O5 content of 6% by weight, of which 15% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to the metal element of Group VIII is 1:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 28.0 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature increases by 3.2°C after 5 days of reaction.
[0092] Comparative Example 3
[0093] A certain amount of MoO3, basic cobalt carbonate, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape. Comparative Example 3 selected the phosphorus-containing alumina carrier in Example 1.
[0094] The prepared catalyst has a MoO3 content of 20% by weight, an atomic ratio of (Co+Ni) / (Co+Ni+Mo) of 0.3, an atomic ratio of Co / (Co+Ni) of 0.5, and a P2O5 content of 6% by weight, of which 15% by weight of P2O5 comes from the carrier. The molar ratio of propylene glycol to Group VIII metal is 1:1. After the catalyst is sulfurized and reacted, the sulfur content in the product is 26.5 ppm. When the sulfur content of the product is maintained at 10 ppm, the reaction temperature rises by 2.9°C after 5 days of reaction.
[0095] Comparative Example 4
[0096] The catalyst was prepared according to the method of Example 3, except that no organic alcohol compound was introduced during the preparation process. After the catalyst was sulfurized and tested for reaction, the sulfur content of the product was 42.6 ppm. When the sulfur content of the product was kept at 10 ppm, the reaction temperature increased by 3.6° C. after 5 days of reaction.
[0097] Comparative Example 5
[0098] The catalyst was prepared according to the method of Example 2, except that the phosphorus content in the catalyst was 1.2% by weight, calculated as P2O5. After the catalyst was sulfurized and tested for reaction, the sulfur content in the product was 38.9 ppm. When the sulfur content of the product was kept at 10 ppm, the reaction temperature increased by 3.6°C after 5 days of reaction.
[0099] It can be seen from the examples and comparative examples that the catalyst provided by the present invention has high activity and stability under low-pressure reaction conditions, has excellent hydrodesulfurization performance under low-pressure reaction conditions, and has good industrial application prospects.
[0100] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrodesulfurization catalyst suitable for low pressure conditions, the catalyst comprising at least one metal element of Group VIII, at least one metal element of Group VIB, phosphorus, an alumina carrier and at least one organic alcohol compound and / or a carboxylic acid compound; wherein: The phosphorus content in the catalyst is 2-10% by weight, calculated as P2O5; Wherein, based on the total amount of the catalyst, the content of the metal element of Group VIB is 12-28% by weight in terms of oxide; wherein, calculated as the element, the atomic ratio of cobalt in the Group VIII metal elements to the total amount of the Group VIII metal elements is not less than 0.8; The alumina carrier contains phosphorus, and the phosphorus in the alumina carrier accounts for 10-40% by weight of the total phosphorus content in the catalyst, calculated as P2O5; The water absorption rate of the alumina carrier is greater than 0.9 mL / g, and the specific surface area is greater than 260 m 2 / g, average pore size greater than 10nm; Wherein, in the alumina carrier, the volume of pores with a pore size distribution of 2-6 nm accounts for no more than 10% of the total pore volume of the alumina carrier; Wherein, in the alumina carrier, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 4% of the total pore volume of the alumina carrier.
2. The catalyst according to claim 1, wherein The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element is 0.1-0.35:
1.
3. The catalyst according to claim 2, wherein The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element is 0.2-0.3:
1.
4. The catalyst according to claim 1, wherein The phosphorus content in the catalyst is 3-10% by weight, calculated as P2O5.
5. The catalyst according to claim 1, wherein The phosphorus in the alumina support accounts for 10-35% by weight of the total phosphorus content in the catalyst, calculated as P2O5.
6. The catalyst according to claim 1, wherein The precursor of the alumina carrier is pseudo-boehmite, and the pseudo-boehmite contains phosphorus.
7. The catalyst according to claim 1, wherein The sodium oxide content in the pseudo-boehmite does not exceed 0.08% by weight.
8. The catalyst according to claim 7, wherein The sodium oxide content in the pseudo-boehmite does not exceed 0.06% by weight.
9. The catalyst according to claim 1, wherein In the alumina carrier, the volume of pores with pore diameter distribution in the range of 2-6 nm accounts for no more than 8% of the total pore volume of the alumina carrier.
10. The catalyst according to claim 1, wherein In the alumina carrier, the volume of pores with pore diameter distribution in the range of 2-4 nm accounts for no more than 2% of the total pore volume of the alumina carrier.
11. The catalyst according to claim 1, wherein The molar ratio of the organic alcohol compound and / or carboxylic acid compound to the metal element of Group VIII is 0.5-6:
1.
12. The catalyst according to claim 11, wherein The molar ratio of the organic alcohol compound and / or the carboxylic acid compound to the metal element of Group VIII is 1-5:
1.
13. The catalyst according to claim 1, wherein The organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane.
14. The catalyst according to claim 13, wherein The organic alcohol compound is at least one of glycerol, propanol and ethylene glycol.
15. The catalyst according to claim 1, wherein The carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid.
16. The catalyst according to claim 15, wherein The carboxylic acid compound is at least one of formic acid, citric acid and acetic acid.
17. The catalyst according to any one of claims 1 to 16, wherein The equivalent diameter of the catalyst is 0.5-1.8 mm.
18. The catalyst according to claim 17, wherein The equivalent diameter of the catalyst is 0.8-1.6 mm.
19. The catalyst according to any one of claims 1 to 16, wherein The catalyst is in the shape of a cylinder, a three-leaf clover, a four-leaf clover, a butterfly, a honeycomb or other irregular shapes.
20. A method for preparing a hydrodesulfurization catalyst suitable for low pressure conditions according to any one of claims 1 to 19, the method comprising: The metal precursor of Group VIII, the metal precursor of Group VIB, the phosphorus-containing compound and the organic alcohol compound and / or the carboxylic acid compound are introduced into the alumina carrier by an impregnation method, and then dried.
21. The preparation method according to claim 20, wherein: The impregnation method comprises: impregnating the aluminum oxide with an impregnation solution containing a Group VIII metal precursor, a Group VIB metal precursor, a phosphorus-containing compound, and an organic alcohol compound and / or a carboxylic acid compound.
22. The preparation method according to claim 21, wherein The organic alcohol compound and / or carboxylic acid compound, the Group VIII metal precursor, and the Group VIB metal precursor are respectively added into an aqueous solution of a phosphorus-containing compound to provide the impregnation solution.
23. The preparation method according to claim 20, wherein: The drying conditions include: temperature of 80-200° C. and time of 1-10 h.
24. Use of the hydrodesulfurization catalyst suitable for low pressure conditions according to any one of claims 1 to 19 in distillate oil hydrorefining.
25. The use according to claim 24, wherein: The catalyst is sulfided and converted into a sulfided catalyst before use.