Silicone rubber containing benzocyclobutene group and preparation method thereof

By introducing benzocyclobutene groups into silicone rubber for cross-linking polymerization, the problems of scorch, toxic catalyst residues and high equipment requirements of the existing silicone rubber cross-linking system are solved, and efficient and safe preparation of silicone rubber is achieved. , has excellent high and low temperature resistance and mechanical properties.

CN118930908AActive Publication Date: 2024-11-12DONGHUA UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411170670.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing silicone rubber crosslinking system has defects such as scorch problems, toxic catalyst residues, long crosslinking time and high equipment requirements, making it difficult to meet the needs of high efficiency, safety and easy production.

Method used

Using the preparation method of silicone rubber containing benzocyclobutylene groups, cross-linking polymerization is carried out by the benzocyclobutylene group on the silicone main chain, cross-linking is achieved by heating, avoiding the generation of small molecule by-products, and simplifying the process and open ring polymerization in the presence of base catalyst and polar solvent.

Benefits of technology

It realizes efficient cross-linking of silicone rubber, has good high and low temperature resistance and mechanical properties, simplifies production process, reduces equipment requirements, and does not require initiators, and controllable reactions. The generated silicone rubber has excellent glass transition Temperature and thermal weight loss performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930908A_ABST
    Figure CN118930908A_ABST
Patent Text Reader

Abstract

The invention relates to silicone rubber containing benzocyclobutene groups and a preparation method of the silicone rubber, raw silicone rubber is plastified and mixed and then cured and crosslinked to obtain a cured product, namely the silicone rubber containing the benzocyclobutene groups. The raw silicone rubber has a siloxane main chain, and the siloxane main chain contains a benzocyclobutene group directly connected with a silicon atom; the proportion of a repeating unit containing a benzocyclobutene group in the siloxane main chain is 0.1-5%; the glass transition temperature of the prepared silicone rubber containing the benzocyclobutene group is-110 + / -5 DEG C, the 5% thermal weight loss temperature is 450 + / -10 DEG C, the tensile strength is 5.0-6.9 MPa, and the tear strength is 35.34-40.12 kN / m. The preparation method disclosed by the invention is simple, small-molecular impurities are not introduced, and low-molecular byproducts are not generated in the reaction process; the benzocyclobutene group-containing silicone rubber has good high and low temperature resistance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone rubber and relates to silicone rubber containing benzocyclobutene groups and a preparation method thereof. Background Art

[0002] Silicone rubber refers to a straight-chain polysiloxane with both inorganic and organic properties, whose main chain is composed of alternating silicon atoms and oxygen atoms. Since the bond energy of Si-O on the main chain of silicone rubber molecules (460kJ / mol) is greater than the bond energy of CC in ordinary rubber (330kJ / mol), compared with ordinary rubber, it has excellent high and low temperature resistance (working temperature range can reach -100 to 300℃), chemical stability, oxygen aging resistance, ozone aging resistance, light aging resistance, weathering aging resistance, gas permeability, electrical insulation, good mechanical properties, oil resistance, solvent resistance and radiation resistance, and is widely used in aerospace, electronic appliances, chemical instrumentation, machinery manufacturing, construction industry and other fields. In addition, silicone rubber is also used in the medical field because of its physiological inertness, no foreign body reaction after implantation in human tissue, and no inflammation to surrounding tissues.

[0003] The crosslinking system of silicone rubber is an important factor affecting the performance of silicone rubber. The currently reported silicone rubber crosslinking systems mainly include peroxide crosslinking system, hydrosilylation crosslinking system, functional group condensation crosslinking system and radiation-induced crosslinking system. However, these crosslinking systems all have certain defects:

[0004] Reference 1 (Study on the Effect of Triallyl Isocyanurate on General Peroxide Curing System Silicone Rubber [J]. Guangdong Chemical Industry, 2017: 118-119.) points out that the peroxide cross-linking system has a scorching problem, so it is necessary to add a scorching retarder to absorb the molecular chain free radicals generated in the early stage of cross-linking of the rubber material, so as to avoid the excessive cross-linking of the macromolecular chain. Although the addition of scorching retarder can improve the scorching problem, it will also reduce the cross-linking density of silicone rubber and even cause the main chain to break. In addition, it is necessary to add a variety of cross-linking aids for use in combination, and the formula design is complicated.

[0005] Reference 2 (Bis-nitrile and bis-dialkylcyanamide platinum (II) complexes as efficient catalysts for hydrosilylation cross-linking of siloxane polymers [J]. Molecules, 2016: 21030311.) points out that the hydrosilylation cross-linking system requires the addition of a transition metal catalyst, which has certain toxicity. In addition, the catalyst cannot be removed after cross-linking, which will affect the performance of the product and limit the scope of use.

[0006] Reference 3 (Synthesis and characterization of room temperature vulcanized silicone rubber using methoxyl-capped MQ silicone resin as self-reinforced cross-linker [J]. Polymers, 2019: 1142.) points out that the functional group condensation cross-linking system mainly relies on the cross-linking points in the main chain of the molecule to contact moisture in the air to undergo a cross-linking reaction to form a cross-linked structure. The cross-linking time is often long, and the small molecule by-products in the cross-linking process are difficult to remove.

[0007] Reference 4 (Research on Radiation Crosslinking of Silicone Rubber [J]. New Chemical Materials, 2007: 62-64.) points out that the radiation-induced crosslinking system has certain requirements for production equipment, and the crosslinking process is often accompanied by polymer degradation, which can easily lead to uncontrolled vulcanization of silicone rubber.

[0008] Therefore, it is of great significance to study a new silicone rubber cross-linking system and use it to prepare silicone rubber to solve the problems existing in the prior art. Summary of the invention

[0009] The purpose of the present invention is to solve the problems existing in the prior art and provide a silicone rubber containing benzocyclobutene groups and a preparation method thereof.

[0010] A method for preparing silicone rubber containing benzocyclobutene groups, comprising plasticizing and mixing the raw silicone rubber, and then curing and cross-linking the raw silicone rubber to obtain a cured product, namely, the silicone rubber containing benzocyclobutene groups;

[0011] The silicone rubber raw rubber has a siloxane main chain, and the siloxane main chain contains a benzocyclobutene group directly connected to the silicon atom;

[0012] The siloxane main chain has a molecular structure as shown in formula (I):

[0013]

[0014] In the formula, x is a positive integer ≥ 1000, preferably a positive integer of 1000 to 5000; each R1 and R4 are independently selected from the following group:

[0015] (a) H;

[0016] (b) substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl; the substitution means that one or more hydrogen atoms on the group are replaced by one or more of the following substituents: halogen, C1-C4 alkyl, C2-C4 alkenyl, C2-C4 alkynyl, unsubstituted phenyl, 1 to 3 hydrogen atoms on the benzene ring are replaced by halogen or C1-C4 alkyl;

[0017] (c) substituted or unsubstituted phenyl; the substitution means that one or more hydrogen atoms on the group are replaced by one or more of the following substituents: halogen, C1-C4 alkyl, C2-C4 alkenyl, C2-C4 alkynyl, unsubstituted phenyl;

[0018] (d) benzocyclobutenyl;

[0019] Furthermore, at least one of R1 or R4 is a benzocyclobutenyl group.

[0020] The specific synthesis path of silicone rubber raw rubber is as follows Figure 2 As shown, starting from benzocyclobutene (BCB), a silicon-containing benzocyclobutene intermediate Si-BCB is obtained through bromination reaction and Grignard reaction in sequence, and then a four-membered ring silicone intermediate M4-BCB containing a benzocyclobutene group is obtained through hydrolysis reaction, which is polymerized with another monomer octamethylcyclotetrasiloxane (D4) to obtain silicone rubber raw rubber (p-BCB).

[0021] The preparation steps of Br-BCB are as follows:

[0022] (1) To a 500 ml three-necked flask equipped with a constant pressure dropping funnel, 240 ml of water and 23.7 g of benzocyclobutene were added in sequence. After cooling in an ice-water bath, 11.7 ml of liquid bromine was added. The ice-water bath was removed and the reaction was allowed to proceed overnight at room temperature.

[0023] (2) After the reaction in step (1) is completed, 50 ml of n-hexane is added to extract the product of reaction (1), and the reaction is quenched with sodium sulfite. The mixture is stirred until colorless, and the organic layer is obtained by separation. The organic layer is then dried over anhydrous sodium sulfate and filtered. The solvent (n-hexane) is then evaporated and n-hexane is added as the mobile phase to pass through the column.

[0024] The preparation steps of Si-BCB are as follows:

[0025] (I) Add an appropriate amount of magnesium chips into a 250 mL beaker, wash with 10 wt % dilute hydrochloric acid three times, then wash with distilled water three times, wash with anhydrous acetone three times, wash with anhydrous ether three times, then filter, and finally dry the magnesium chips in a vacuum oven at 55° C. overnight to obtain activated magnesium chips;

[0026] (II) Under N2 protection, 2.7 g of activated magnesium chips, 70 ml of tetrahydrofuran, 24.5 g of methyltriethoxysilane and two iodine particles were added to a 250 ml three-necked flask equipped with a reflux condenser and a constant pressure dropping funnel. After heating to reflux at 70°C, a mixed solution of 20 ml of tetrahydrofuran and 10 g of 4-bromobenzocyclobutene was added. After the addition was completed, the mixture was incubated for 1 hour and refluxed for 16 hours.

[0027] (III) After the reaction of step (II) is completed, the mixture is cooled to room temperature, filtered through diatomaceous earth, and then tetrahydrofuran and methyltriethoxysilane are distilled off under reduced pressure, and finally the target product Si-BCB is obtained by distillation under reduced pressure. The structural formula of Si-BCB is Boiling point Bp of Si-BCB: 103~110℃ (20mmHg).

[0028] The raw silicone rubber of the invention can be cross-linked and polymerized by heating, and no small molecular by-products are generated during the cross-linking process. The cured cross-linked product has good high and low temperature resistance and mechanical properties.

[0029] The specific steps of preparing silicone rubber containing benzocyclobutene groups from silicone rubber raw rubber are as follows:

[0030] (1) Plasticizing and mixing: Add 100 parts of p-BCB on a double-roll open mill at 45°C and a roll gap of 1.0 mm, then add 30 parts of fumed silica (particle size 7-40 nm) in three times and mix for 0.5-1 h. Remove the rubber and leave it at room temperature for 2-3 h, then mix it a second time (re-mix).

[0031] (2) Curing and cross-linking: The rubber material after the reaction in step (1) is placed in the prepared mold and placed in a preheated flat vulcanizer for multiple exhausts and vulcanized at 180°C for 30 minutes and then at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa.

[0032] As the preferred technical solution:

[0033] In the method for preparing the silicone rubber containing benzocyclobutene groups as described above, the ratio of the repeating units containing benzocyclobutene groups in the siloxane main chain is 0.1-5%, preferably 0.1-1%.

[0034] A method for preparing a silicone rubber containing a benzocyclobutene group as described above, wherein the silicone rubber raw rubber is prepared by ring-opening polymerization of an organic silicon monomer as shown in formula (II) in the presence of an alkali catalyst and a polar solvent;

[0035]

[0036] The method for preparing a silicone rubber containing a benzocyclobutene group as described above, wherein the base catalyst is one or more of sodium hydroxide, potassium hydroxide and tetramethylammonium hydroxide, preferably tetramethylammonium hydroxide;

[0037] The polar solvent is tetrahydrofuran, triethylene glycol dimethyl ether, N,N-dimethylformamide, dimethyl sulfoxide or N-methylpyrrolidone, preferably N-methylpyrrolidone.

[0038] In the method for preparing a silicone rubber containing a benzocyclobutene group as described above, the temperature of the ring-opening polymerization reaction is 50 to 120° C. and the time is 2 to 24 hours.

[0039] In the above-mentioned method for preparing a silicone rubber containing a benzocyclobutene group, the silicone monomer is obtained by hydrolyzing a monomer as shown in formula (III);

[0040]

[0041] In the formula, R2 and R3 are each independently selected from C1-C4 alkoxy and halogen.

[0042] The method for preparing a silicone rubber containing a benzocyclobutene group as described above, wherein the hydrolysis reaction is carried out in the presence of an acid catalyst and a solvent, the reaction temperature is 25 to 55° C., and the reaction time is 2 to 12 hours;

[0043] The acid catalyst is a hydrochloric acid solution, a sulfuric acid solution or an acetic acid solution with a concentration of 4 to 6 mol / L, preferably a hydrochloric acid solution with a concentration of 6 mol / L;

[0044] The solvent is benzene, toluene or xylene, preferably toluene.

[0045] The reaction equation is:

[0046]

[0047] The present invention also provides a silicone rubber containing benzocyclobutene groups prepared by the preparation method described in any one of the above items, wherein the glass transition temperature (T g ) is -110±5°C, 5% thermal weight loss temperature is 450±10°C, tensile strength is 5.0-6.9MPa, tear strength is 35.34-40.12kN / m, and elongation at break is 500-1000%. The invention provides a new cross-linking system for silicone rubber, which is simple and easy to operate, and the reaction is controllable. The obtained cured product has good high and low temperature resistance and mechanical properties.

[0048] Beneficial effects:

[0049] (1) The method for preparing a silicone rubber containing a benzocyclobutene group of the present invention does not require the addition of an initiator, and the cross-linking of the silicone rubber can be achieved only by heating, and no small molecular impurities are introduced. No low molecular weight byproducts are generated during the reaction, and the reaction is controllable and has low requirements on production equipment;

[0050] (2) The method for preparing a silicone rubber containing a benzocyclobutene group of the present invention is a new method for vulcanizing raw silicone rubber, which is simple and easy to operate, and the reaction is controllable;

[0051] (4) The silicone rubber containing benzocyclobutene groups of the present invention has good high and low temperature resistance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 The thermal cross-linking mechanism of benzocyclobutene;

[0053] Figure 2 This is the synthetic route of silicone rubber (p-BCB). DETAILED DESCRIPTION

[0054] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0055] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:

[0056] 5% thermal weight loss temperature: TA Discovery TGA 550 analyzer was used to test the sample using 5 mg at a heating rate of 10°C / min from room temperature to 800°C with a nitrogen flow rate of 60 mL / min.

[0057] Tensile strength and elongation at break: According to GB / T 528-2009, dumbbell-shaped test specimens were used, and the test was carried out at a speed of 500 mm / min using a UTM 2502 microcomputer-controlled electronic universal testing machine under a 50N load cell.

[0058] Tear strength: According to GB / T 529-2008, a rectangular test specimen was used, and the test was carried out at a speed of 500 mm / min using a UTM2502 microcomputer-controlled electronic universal testing machine under a 50N load cell.

[0059] Example 1

[0060] A method for preparing silicone rubber containing benzocyclobutene groups, the specific steps are as follows:

[0061] (1) Preparation of organosilicon monomer I;

[0062] (1.1) Add 30 ml of 6 mol / L hydrochloric acid solution and 15 ml of toluene to a 250 ml three-necked flask equipped with a constant pressure dropping funnel, then add 15 ml of toluene, 2.36 g and 3.61g After the addition of the mixed solution, the temperature was raised to 50°C and the hydrolysis reaction was carried out for 6 hours;

[0063] (1.2) After the reaction in step (1.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (toluene) is evaporated to obtain organosilicon monomer I, namely M4-BCB:

[0064] (2) Preparation of organosilicon monomer II;

[0065] (2.1) Add 120 ml of 6 mol / L hydrochloric acid solution and 60 ml of toluene to a 500 ml three-necked flask equipped with a constant pressure dropping funnel, then add 60 ml of toluene and 19.24 g of After the addition of the mixed solution, the temperature was raised to 50°C and the hydrolysis reaction was carried out for 6 hours;

[0066] (2.2) After the reaction in step (2.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (toluene) is evaporated to obtain organosilicon monomer II, i.e., octamethylcyclotetrasiloxane:

[0067] (3) Preparation of silicone rubber;

[0068] (3.1) Preparation of TMAS: 0.2 g of tetramethylammonium hydroxide (TMAH) and 10 g of octamethylcyclotetrasiloxane (D4) were added to a 100 ml round-bottom flask, and the mixture was vacuumed at 55 °C for 1 h, water was removed, and the mixture was heated to 65 °C and reacted for 3 h to obtain an off-white viscous liquid, i.e., TMAS.

[0069] (3.2) 0.0618 g of M4-BCB and 11.8648 g of D4 were added to a 100 ml three-necked flask, and the mixture was vacuumed at 55°C for 1 h to remove water. 0.2398 g of alkali rubber and 0.1847 g of N-methylpyrrolidone (NMP) were added, and the polymerization reaction was carried out at 75°C for 8 h to obtain silicone rubber (p-BCB).

[0070] The number average molecular weight (Mn) of the prepared silicone rubber is 2.33×10 5 , the weight average molecular weight (Mw) is 4.45×10 5; Silicone rubber has a siloxane main chain, which contains benzocyclobutene groups directly connected to silicon atoms; the molecular structure of the siloxane main chain is as follows: n and m are positive integers; the proportion of repeating units containing benzocyclobutene groups in the siloxane main chain is 0.1%.

[0071] (4) After plasticizing and mixing the raw silicone rubber for 1 hour, the rubber is taken out and placed at room temperature for 2 hours, and then the rubber is mixed for a second time. Finally, it is vulcanized on a flat vulcanizer at 180°C for 30 minutes and at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa to obtain a cured product, i.e., silicone rubber containing benzocyclobutene groups.

[0072] The glass transition temperature of the cyclobutene-group silicone rubber finally obtained is -108°C, the 5% thermal weight loss temperature is 449°C, the tensile strength is 5MPa, the tear strength is 35.34kN / m, and the elongation at break is 500%.

[0073] Example 2

[0074] A method for preparing silicone rubber containing benzocyclobutene groups, the specific steps are as follows:

[0075] (1) Preparation of organosilicon monomer I;

[0076] (1.1) Add 30 ml of 6 mol / L hydrochloric acid solution and 15 ml of benzene to a 250 ml three-necked flask equipped with a constant pressure dropping funnel, then add 15 ml of benzene, 2.36 g and 4.45g After the addition of the mixed solution, the temperature was raised to 55°C and the hydrolysis reaction was carried out for 4 hours;

[0077] (1.2) After the reaction in step (1.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (benzene) is evaporated to obtain organosilicon monomer I, namely M4-BCB:

[0078] (2) Preparation of organosilicon monomer II;

[0079] (2.1) Add 120 ml of 6 mol / L hydrochloric acid solution and 60 ml of benzene to a 500 ml three-necked flask equipped with a constant pressure dropping funnel, then add 60 ml of benzene and 23.72 g of After the addition of the mixed solution, the temperature was raised to 55°C and the hydrolysis reaction was carried out for 4 hours;

[0080] (2.2) After the reaction in step (2.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (benzene) is evaporated to obtain organosilicon monomer II, i.e., octamethylcyclotetrasiloxane:

[0081] (3) Preparation of silicone rubber;

[0082] (3.1) Preparation of TMAS: 0.2 g of sodium hydroxide and 10 g of octamethylcyclotetrasiloxane (D4) were added to a 100 ml round-bottom flask, and the mixture was vacuumed at 55 °C for 1 h, water was removed, and the mixture was heated to 65 °C and reacted for 3 h to obtain an off-white viscous liquid, i.e., TMAS.

[0083] (3.2) 0.25 g of M4-BCB and 11.8648 g of D4 were added to a 100 ml three-necked flask, and the mixture was vacuumed at 55°C for 1 h to remove water. 0.2423 g of alkali rubber and 0.1866 g of N-methylpyrrolidone (NMP) were added and ring-opening polymerization was carried out at 85°C for 6 h to obtain silicone rubber raw rubber, i.e. silicone rubber containing benzocyclobutene groups.

[0084] The number average molecular weight (Mn) of the prepared silicone rubber is 2.13×10 5 The weight average molecular weight (Mw) is 4.66×10 5 ; Silicone rubber has a siloxane main chain, which contains benzocyclobutene groups directly connected to silicon atoms; the molecular structure of the siloxane main chain is as follows: n and m are positive integers; the proportion of repeating units containing benzocyclobutene groups in the siloxane main chain is 0.4%.

[0085] (4) After plasticizing and mixing the raw silicone rubber for 1 hour, the rubber material is removed and placed at room temperature for 2 hours, and then mixed for a second time. Finally, the rubber material is vulcanized on a flat vulcanizer at 180°C for 30 minutes and at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa to obtain a cured product, i.e., a cyclobutene-group silicone rubber.

[0086] The glass transition temperature of the cyclobutene-group silicone rubber finally obtained is -110°C, the 5% thermal weight loss temperature is 454°C, the tensile strength is 6.9 MPa, the tear strength is 40.12 kN / m, and the elongation at break is 1000%.

[0087] Example 3

[0088] A method for preparing silicone rubber containing benzocyclobutene groups, the specific steps are as follows:

[0089] (1) Preparation of organosilicon monomer I;

[0090] (1.1) Add 30 ml of 4 mol / L acetic acid solution and 15 ml of xylene to a 250 ml three-necked flask equipped with a constant pressure dropping funnel, then add 15 ml of xylene, 2.36 g and 3.61g After the addition of the mixed solution, the temperature was raised to 40°C and the hydrolysis reaction was carried out for 12 hours;

[0091] (1.2) After the reaction in step (1.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (xylene) is evaporated to obtain organosilicon monomer I, namely M4-BCB:

[0092] (2) Preparation of organosilicon monomer II;

[0093] (2.1) Add 120 ml of 4 mol / L acetic acid solution and 60 ml of xylene to a 500 ml three-necked flask equipped with a constant pressure dropping funnel, then add 60 ml of xylene and 19.24 g of After the addition of the mixed solution, the temperature was raised to 40°C and the hydrolysis reaction was carried out for 12 hours;

[0094] (2.2) After the reaction in step (2.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (xylene) is evaporated to obtain organosilicon monomer II, i.e., octamethylcyclotetrasiloxane:

[0095] (3) Preparation of silicone rubber;

[0096] (3.1) Preparation of TMAS: 0.2 g potassium hydroxide and 10 g octamethylcyclotetrasiloxane (D4) were added to a 100 ml round-bottom flask, and the mixture was vacuumed at 55 °C for 1 h, water was removed, and the mixture was heated to 65 °C and reacted for 3 h to obtain an off-white viscous liquid, i.e. TMAS.

[0097] (3.2) 0.615 g of M4-BCB and 11.8648 g of D4 were added to a 100 ml three-necked flask, and the mixture was vacuumed at 55 °C for 1 h to remove water. 0.2496 g of alkali rubber and 0.3454 g of triethylene glycol dimethyl ether were added, and a ring-opening polymerization reaction was carried out at 90 °C for 5 h to obtain raw silicone rubber.

[0098] The number average molecular weight (Mn) of the prepared silicone rubber is 2.01×10 5 The weight average molecular weight (Mw) is 4.55×10 5 ; Silicone rubber has a siloxane main chain, which contains benzocyclobutene groups directly connected to silicon atoms; the molecular structure of the siloxane main chain is as follows: n and m are positive integers; the proportion of repeating units containing benzocyclobutene groups in the siloxane main chain is 1%.

[0099] (4) After plasticizing and mixing the raw silicone rubber for 1 hour, the rubber is taken out and placed at room temperature for 2 hours, and then the rubber is mixed for a second time. Finally, it is vulcanized on a flat vulcanizer at 180°C for 30 minutes and at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa to obtain a cured product, i.e., silicone rubber containing benzocyclobutene groups.

[0100] The glass transition temperature of the cyclobutene-group silicone rubber finally obtained is -107°C, the 5% thermal weight loss temperature is 442°C, the tensile strength is 5.5 MPa, the tear strength is 38.63 kN / m, and the elongation at break is 800%.

[0101] Example 4

[0102] A method for preparing silicone rubber containing benzocyclobutene groups, the specific steps are as follows:

[0103] (1) Preparation of organosilicon monomer I;

[0104] (1.1) Add 30 ml of 4 mol / L hydrochloric acid solution and 15 ml of toluene to a 250 ml three-necked flask equipped with a constant pressure dropping funnel, then add 15 ml of toluene, 2.36 g and 4.45g After the addition of the mixed solution, the temperature was raised to 45°C and the hydrolysis reaction was carried out for 8 hours;

[0105] (1.2) After the reaction in step (1.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (toluene) is evaporated to obtain organosilicon monomer I, namely M4-BCB:

[0106] (2) Preparation of organosilicon monomer II;

[0107] (2.1) Add 120 ml of 4 mol / L hydrochloric acid solution and 60 ml of toluene to a 500 ml three-necked flask equipped with a constant pressure dropping funnel, then add 60 ml of toluene and 23.72 g of After the addition of the mixed solution, the temperature was raised to 45°C and the hydrolysis reaction was carried out for 8 hours;

[0108] (2.2) After the reaction in step (2.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (toluene) is evaporated to obtain organosilicon monomer II, i.e., octamethylcyclotetrasiloxane:

[0109] (3) Preparation of silicone rubber;

[0110] (3.1) Preparation of TMAS: 0.2 g of tetramethylammonium hydroxide and 10 g of octamethylcyclotetrasiloxane (D4) were added to a 100 ml round-bottom flask, and the mixture was vacuumed at 55 °C for 1 h, water was removed, and the mixture was heated to 65 °C and reacted for 3 h to obtain an off-white viscous liquid, i.e., TMAS.

[0111] (3.2) 2.09 g of M4-BCB and 11.8648 g of D4 were added to a 100 ml three-necked flask, and the mixture was vacuumed at 55 °C for 1 h to remove water. 0.2791 g of alkali rubber and 0.1585 g of N,N-dimethylformamide were added, and a ring-opening polymerization reaction was carried out at 100 °C for 4 h to obtain raw silicone rubber.

[0112] The number average molecular weight (Mn) of the obtained silicone rubber is 2.23×10 5 , the weight average molecular weight (Mw) is 4.50×10 5 ; Silicone rubber has a siloxane main chain, which contains benzocyclobutene groups directly connected to silicon atoms; the molecular structure of the siloxane main chain is as follows: n and m are positive integers; the proportion of repeating units containing benzocyclobutene groups in the siloxane main chain is 3%.

[0113] (4) After plasticizing and mixing the raw silicone rubber for 1 hour, the rubber is taken out and placed at room temperature for 2 hours, and then the rubber is mixed for a second time. Finally, it is vulcanized on a flat vulcanizer at 180°C for 30 minutes and at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa to obtain a cured product, i.e., silicone rubber containing benzocyclobutene groups.

[0114] The glass transition temperature of the cyclobutene-group silicone rubber finally obtained is -106°C, the 5% thermal weight loss temperature is 450°C, the tensile strength is 5.8MPa, the tear strength is 39.45kN / m, and the elongation at break is 900%.

[0115] Example 5

[0116] A method for preparing silicone rubber containing benzocyclobutene groups, the specific steps are as follows:

[0117] (1) Preparation of organosilicon monomer I;

[0118] (1.1) Add 30 ml of 5 mol / L sulfuric acid solution and 15 ml of xylene to a 250 ml three-necked flask equipped with a constant pressure dropping funnel, then add 15 ml of xylene, 2.36 g and 4.45g After the addition of the mixed solution, the temperature was raised to 30°C and the hydrolysis reaction was carried out for 12 hours;

[0119] (1.2) After the reaction in step (1.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (xylene) is evaporated to obtain organosilicon monomer I, namely M4-BCB:

[0120] (2) Preparation of organosilicon monomer II;

[0121] (2.1) Add 120 ml of 5 mol / L sulfuric acid solution and 60 ml of xylene to a 500 ml three-necked flask equipped with a constant pressure dropping funnel, then add 60 ml of xylene and 23.72 g of After the addition of the mixed solution, the temperature was raised to 30°C and the hydrolysis reaction was carried out for 12 hours;

[0122] (2.2) After the reaction in step (2.1) is completed, the mixture is washed with deionized water until neutral, separated, the organic phase is dried with anhydrous sodium sulfate, filtered, and the solvent (xylene) is evaporated to obtain organosilicon monomer II, i.e., octamethylcyclotetrasiloxane:

[0123] (3) Preparation of silicone rubber;

[0124] (3.1) Preparation of TMAS: 0.2 g of a mixture of potassium hydroxide and tetramethylammonium hydroxide in a mass ratio of 1:1 and 10 g of octamethylcyclotetrasiloxane (D4) were added to a 100 ml round-bottom flask, and vacuumed at 55 °C for 1 h, water was removed, and the temperature was raised to 65 °C and reacted for 3 h to obtain an off-white viscous liquid, i.e., TMAS.

[0125] (3.2) 3.8473 g of M4-BCB and 11.8648 g of D4 were added to a 100 ml three-necked flask, and the mixture was vacuumed at 55°C for 1 h to remove water. 0.3142 g of alkali rubber and 0.1907 g of dimethyl sulfoxide were added, and a ring-opening polymerization reaction was carried out at 120°C for 2 h to obtain raw silicone rubber.

[0126] The number average molecular weight (Mn) of the prepared silicone rubber is 2.09×10 5 The weight average molecular weight (Mw) is 4.49×10 5 ; Silicone rubber has a siloxane main chain, which contains benzocyclobutene groups directly connected to silicon atoms; the molecular structure of the siloxane main chain is as follows: n and m are positive integers; the proportion of repeating units containing benzocyclobutene groups in the siloxane main chain is 5%.

[0127] (4) After plasticizing and mixing the raw silicone rubber for 1 hour, the rubber is taken out and placed at room temperature for 2 hours, and then the rubber is mixed for a second time. Finally, it is vulcanized on a flat vulcanizer at 180°C for 30 minutes and at 200°C for 3 hours. The entire vulcanization process is completed at a pressure of 8 MPa to obtain a cured product, i.e., silicone rubber containing benzocyclobutene groups.

[0128] The glass transition temperature of the cyclobutene-group silicone rubber finally obtained was -105°C, the 5% thermal weight loss temperature was 455°C, the tensile strength was 5.3 MPa, the tear strength was 39.6 kN / m, and the elongation at break was 600%.

Claims

1. A method for preparing a silicone rubber containing a benzocyclobutene group, characterized in that: After plasticizing and mixing the raw silicone rubber, curing and cross-linking are performed to obtain a cured product, namely, silicone rubber containing benzocyclobutene groups; The silicone rubber raw rubber has a siloxane main chain, and the siloxane main chain contains a benzocyclobutene group directly connected to the silicon atom; The siloxane main chain has a molecular structure as shown in formula (I): Wherein, x is a positive integer ≥1000; each R1 and R4 are independently selected from the following group: (a) H; (b) substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl; the substitution means that one or more hydrogen atoms on the group are replaced by one or more of the following substituents: halogen, C1-C4 alkyl, C2-C4 alkenyl, C2-C4 alkynyl, unsubstituted phenyl, 1 to 3 hydrogen atoms on the benzene ring are replaced by halogen or C1-C4 alkyl; (c) substituted or unsubstituted phenyl; the substitution means that one or more hydrogen atoms on the group are replaced by one or more of the following substituents: halogen, C1-C4 alkyl, C2-C4 alkenyl, C2-C4 alkynyl, unsubstituted phenyl; (d) benzocyclobutenyl; Furthermore, at least one of R1 or R4 is a benzocyclobutenyl group.

2. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 1, characterized in that: The proportion of repeating units containing benzocyclobutene groups in the main chain of the siloxane is 0.1-5%.

3. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 1, characterized in that: The silicone rubber raw rubber is prepared by ring-opening polymerization of an organic silicon monomer as shown in formula (II) in the presence of an alkali catalyst and a polar solvent; 4. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 3, characterized in that: The alkaline catalyst is one or more of sodium hydroxide, potassium hydroxide and tetramethylammonium hydroxide; The polar solvent is tetrahydrofuran, triethylene glycol dimethyl ether, N,N-dimethylformamide, dimethyl sulfoxide or N-methylpyrrolidone.

5. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 3, characterized in that: The temperature of the ring-opening polymerization reaction is 50-120° C., and the time is 2-24 hours.

6. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 3, characterized in that: The organosilicon monomer is obtained by hydrolysis reaction of the monomer represented by formula (III); In the formula, R2 and R3 are each independently selected from C1-C4 alkoxy and halogen.

7. The method for preparing a silicone rubber containing benzocyclobutene groups according to claim 6, characterized in that: The hydrolysis reaction is carried out in the presence of an acid catalyst and a solvent, the reaction temperature is 25 to 55° C., and the reaction time is 2 to 12 hours; The acid catalyst is a hydrochloric acid solution, a sulfuric acid solution or an acetic acid solution with a concentration of 4 to 6 mol / L; The solvent is benzene, toluene or xylene.

8. The silicone rubber containing benzocyclobutene groups prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The glass transition temperature of the silicone rubber containing benzocyclobutene groups is -110±5°C, the 5% thermal weight loss temperature is 450±10°C, the tensile strength is 5.0-6.9MPa, the tear strength is 35.34-40.12kN / m, and the elongation at break is 500-1000%.

Citation Information

Patent Citations

  • Organosiloxane containing benzocyclobutene group as well as preparation method and application thereof

    CN104356390A

  • Polysilsesquioxane containing benzocyclobutene functional group and preparation method thereof

    CN106432729A

  • Benzocyclobutene functional organic silicone resin and preparation method thereof

    CN107987278A

  • Preparation and application of organo-siloxane capable of being subjected to direct thermal curing

    CN108299645A

  • Room temperature vulcanized silicone rubber cross-linking agent preparation method, and applications thereof

    CN109384958A