Etherification reaction catalyst and preparation method thereof and process for preparing ethylene glycol mono-tert-butyl ether
Through the etherification catalyst of modified resin and amorphous silicon aluminum, the problems of high isobutene content and high by-products in the monotert-butyl ether process of ethylene glycol are solved, which improves the selectivity and process efficiency of ETB and reduces energy Consumption.
Patent Information
- Application Number
- CN202111273198.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The current ethylene glycol monotert-butyl ether process has a high demand for isobutylene content, the proportion of by-product diisobutylene isobutylene, and the selectivity of ETBs is low, resulting in complex processes, high investment and energy consumption.
Using a mixture of modified resin and amorphous silicon-aluminum as the etherification reaction catalyst, the modified resin is heat treatment and calcination, and the contact reaction of ethylene glycol, isobutene and methyl tert-butyl ether under the etherification reaction conditions is reduced. The minimum content of isobutene is required to improve the selectivity of ETB.
It reduces the amount of by-products, improves the selectivity of ETB, simplifies the product separation steps, reduces energy consumption, and broadens the source of raw materials.
Smart Images

Figure CN116060127B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of petrochemical industry, and in particular, to an etherification reaction catalyst and a preparation method thereof, as well as a process for preparing ethylene glycol mono-tert-butyl ether. Background Art
[0002] Ethylene glycol butyl ether is a solvent with excellent performance. It is used as a solvent because of its two strong dissolving groups in its chemical structure. According to foreign studies on toxicity, ethylene glycol methyl (ethyl) ether can be converted into methyl (ethyl) acetic acid in the human body, which has a barrier effect on metabolic function, thereby affecting the bone marrow, lymphatic tissue and developing fetus of animals. The toxicity of ethylene glycol butyl ether to the reproductive system is also recognized, so developed countries abroad have begun to restrict its production and use.
[0003] Compared with ethylene glycol butyl ether, ethylene glycol mono-tert-butyl ether (ETB) has the advantages of high volatility, low odor, low toxicity, low photochemical reactivity, mild skin irritation, good solubility in water, and good dispersion stability in latex coatings. Therefore, it is used as a substitute for ethylene glycol ether.
[0004] ETB is an environmentally friendly alcohol ether solvent, but the common problems in its preparation technology are: (1) liquefied petroleum gas with an isobutylene content of 30% to 100% can be used, but liquefied petroleum gas with an isobutylene content of less than 20% cannot be used; (2) the selectivity of ETB in the product is low; (3) the selectivity of the by-product diisobutylene is high; (4) the low selectivity of ETB in the product leads to more impurities, which in turn affects the separation process, resulting in a complex process and high investment and energy consumption. Summary of the invention
[0005] The purpose of the present disclosure is to solve the problems in the prior art of high isobutylene content requirement in the ethylene glycol tert-butyl ether process, too high proportion of dimerized olefin products in the product, and low selectivity of ETB in the product.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a method for preparing an etherification reaction catalyst, wherein the etherification reaction catalyst comprises a mixture of a modified resin and amorphous silica-alumina; the method comprises the following steps of preparing the modified resin: under protective atmosphere conditions, an organic sulfone and an acidic ion exchange resin are contacted at 50 to 200° C. for heat treatment, and a liquid material is separated and removed from the obtained mixture to obtain a heat-treated resin; and the heat-treated resin is contacted with an organic solvent and then calcined to obtain a modified resin.
[0007] Optionally, the organic sulfone has 2 to 10 carbon atoms; preferably, the organic sulfone is selected from one or more of dimethyl sulfone, methyl vinyl sulfone, cyclobutane sulfone, cyclopentane sulfone, diethyl sulfone and allyl sulfone, and more preferably one or more of dimethyl sulfone, cyclobutane sulfone and allyl sulfone.
[0008] Optionally, the protective atmosphere is selected from one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide, preferably nitrogen.
[0009] Optionally, the heat treatment conditions include a pressure of 0.1 to 20.0 MPa, a temperature of 80 to 150° C., and a time of 0.5 to 20 h; relative to 1 g of the acidic ion exchange resin, the amount of the organic sulfone is 0.5 to 2.5 mL.
[0010] Optionally, the organic solvent includes one or more of ethanol, n-propanol, n-butanol, isopropanol, isobutanol, sec-butanol and tert-butanol, preferably ethanol.
[0011] Optionally, the method comprises: soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then performing the calcination; the soaking temperature is 10 to 50°C and the time is 3 to 10 hours; the calcination temperature is 70 to 120°C and the time is 1 to 5 hours.
[0012] Optionally, the acidic ion exchange resin is selected from a strong acidic ion exchange resin and / or a weak acidic ion exchange resin, preferably a macroporous strong acidic ion exchange resin.
[0013] Optionally, the amorphous silicon-aluminum contains 0 to 0.3 wt % of Na 2 O, 50 to 80% by weight of SiO 2 and 20-50 wt% Al 2 O 3 , where Na 2 O、SiO 2 and Al 2 O 3 The content is measured by XRF method; in the XRD spectrum of the amorphous silicon aluminum, only a diffuse diffraction peak appears at 25°~27°, the most probable pore size of the amorphous silicon aluminum is 20~50nm, and x / y is 0.55~0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XRF method.
[0014] Optionally, the method further comprises mixing the modified resin and the amorphous silica-alumina to obtain the etherification reaction catalyst.
[0015] Optionally, based on dry weight, the mass ratio of the modified resin to the amorphous silicon-alumina is (0.3-3.0):1.
[0016] Optionally, the average particle size of the modified resin is 350-1250 μm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
[0017] In a second aspect of the present disclosure, an etherification reaction catalyst is prepared by the method described in the first aspect of the present disclosure.
[0018] The third aspect of the present disclosure provides a process for preparing ethylene glycol mono-tert-butyl ether, which comprises: under etherification reaction conditions, contacting ethylene glycol, a C4 olefin raw material containing isobutylene and methyl tert-butyl ether under the catalysis of the etherification reaction catalyst described in the second aspect of the present disclosure.
[0019] Optionally, the mass fraction of isobutylene in the C4 olefin feedstock is 5 to 100%, preferably 10 to 100%; the molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin feedstock to the ethylene glycol is 1:1 to 10, preferably 1:2 to 4.
[0020] Optionally, the method further includes adding an additive to the contact reaction, wherein the additive is water and / or alcohol, preferably one or more of water, ethanol, n-propanol, isopropanol and tert-butanol; based on the total weight of the ethylene glycol and the mixed C4 olefins, the weight of the additive is 0.5 to 20% by weight, preferably 2 to 10% by weight.
[0021] Optionally, the etherification reaction conditions include: reaction temperature of 40 to 100°C, preferably 60 to 80°C; reaction pressure of 0.5 to 2.5 MPa, preferably 0.5 to 1.5 MPa; space velocity of 0.1 to 10 h -1 , preferably 0.3~1.0h -1 .
[0022] Optionally, the method further comprises sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit comprises a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.
[0023] Through the above technical scheme, the present invention modifies an acidic ion exchange resin with an organic sulfone to obtain a modified resin, and uses a mixture of the modified resin and amorphous silicon aluminum to prepare an etherification reaction catalyst. The catalyst is used in the reaction of preparing ethylene glycol mono-tert-butyl ether, which can reduce the minimum content requirement of isobutylene in the reaction raw material C4 olefin and broaden the source of raw materials; it can greatly reduce the amount of by-products generated, increase the selectivity for ETB, and thus reduce the energy consumption of the product separation step.
[0024] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0026] Figure 1 It is a process flow chart of a specific implementation mode of the process for preparing ethylene glycol mono-tert-butyl ether disclosed in the present invention.
[0027] Description of Reference Numerals
[0028] 1. Etherification reactor; 2. C4 removal tower; 3. Light removal tower; 4. MTBE removal tower; 5. C8 removal tower; 6. Azeotropic tower; 7. ETB separation tower; 8. Ethylene glycol flash tower; 9. Heavy components; 10. Circulating EG; 11. Circulating EDB; 12. Circulating MTBE; 13. Methanol; 14. ETB product; 15. EG; 16. C4 olefin feedstock; 17. Methyl tert-butyl ether; 18. Mixed C4 materials; 19. C8 logistics. DETAILED DESCRIPTION
[0029] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0030] In the present disclosure, unless otherwise specified, "EG" refers to ethylene glycol, "C4" refers to mixed C4 olefins in the reaction raw materials, "MTBE" refers to methyl tert-butyl ether, "ETB" refers to ethylene glycol mono-tert-butyl ether, "EDB" refers to ethylene glycol di-tert-butyl ether, and "IB" refers to isobutylene. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated.
[0031] The first aspect of the present disclosure provides a method for preparing an etherification reaction catalyst, wherein the etherification reaction catalyst comprises a mixture of a modified resin and amorphous silica-alumina; the method comprises the following steps of preparing the modified resin: under protective atmosphere conditions, contacting an organic sulfone and an acidic ion exchange resin at 50 to 200° C. for heat treatment, separating and removing a liquid material from the obtained mixture to obtain a heat-treated resin; contacting the heat-treated resin with an organic solvent, and then calcining to obtain a modified resin.
[0032] Through the above technical scheme, the preparation method disclosed in the present invention obtains a modified resin by modifying an acidic ion exchange resin with an organic sulfone. The mixture of the modified resin and amorphous silicon aluminum is used as an etherification reaction catalyst to prepare ethylene glycol mono-tert-butyl ether, which can reduce the minimum content requirement of isobutylene in the reaction raw material C4 olefin from 20 weight % to 5 weight %, and at the same time, can reduce the content of isobutylene in the C4 olefin after the etherification reaction, generally can be lower than 3 weight %; can greatly reduce the amount of by-product C8 olefins, etc., generally can be lower than 5 weight %; increase the selectivity of ETB, the selectivity can be as high as 89.5 weight %, and thus can reduce the energy consumption of the product separation step.
[0033] In one embodiment, the method of the present disclosure further comprises subjecting the acidic ion exchange resin to heat treatment in a reactor selected from a stirred tank reactor, a trickle bed reactor and a fixed bed reactor, preferably a fixed bed reactor.
[0034] In one embodiment, the contacting of the acidic ion exchange resin and the organic sulfone for heat treatment under a protective atmosphere may include: pumping the organic sulfone into a reactor under a protective atmosphere, and then adding the acidic ion exchange resin.
[0035] In one embodiment, the organic sulfone has 2 to 10 carbon atoms; preferably, the organic sulfone is selected from one or more of dimethyl sulfone, methyl vinyl sulfone, cyclobutane sulfone, cyclopentane sulfone, diethyl sulfone and allyl sulfone, and more preferably one or more of dimethyl sulfone, cyclobutane sulfone and allyl sulfone.
[0036] In this embodiment, the organic sulfone used is an organic compound containing a sulfone functional group, which can remove moisture from the resin, increase the size of the resin pores, and modify the structure of the resin. The preferred organic sulfone can further enhance the catalytic activity of the modified resin and improve the selectivity of ETB.
[0037] In one embodiment, the protective atmosphere is selected from one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide, preferably nitrogen.
[0038] In this embodiment, the use of protective atmosphere during the modification process can reduce the oxygen content in the acidic ion exchange resin and enhance the modification effect. After the modification is completed, the organic sulfone is pushed out with the protective atmosphere, and then the organic sulfone is swept away with the protective atmosphere to achieve the effect of solid-liquid separation.
[0039] In one embodiment, the organic solvent includes one or more of ethanol, n-propanol, n-butanol, n-pentanol, isopropanol, isobutanol, sec-butanol and tert-butanol, preferably a C2-C5 alcohol, for example, one or more selected from ethanol, n-propanol and n-butanol, more preferably ethanol.
[0040] Contacting the heat-treated resin with an organic solvent may include washing or soaking the heat-treated resin with the organic solvent. The amount of the organic solvent is not particularly limited. For example, the amount of the organic solvent may be 0.1 to 5 mL, preferably 0.5 to 2.5 mL, and more preferably 0.5 to 1.5 mL, relative to 1 g of the heat-treated resin.
[0041] In this embodiment, by soaking the heat-treated resin in an organic solvent, the organic sulfone remaining in the heat-treated resin can be cleaned, and some exchanged impurities in the modified resin can be washed out, thereby enhancing the activity of the modified resin.
[0042] In one embodiment, the heat treatment pressure is 0.1-20.0 MPa, the temperature is 80-150°C, and the time is 0.5-20 h; preferably, the heat treatment pressure is 1.0-5.0 MPa, the temperature is 100-120°C, and the time is 1.5-5.0 h. In this embodiment, the preferred heat treatment conditions can further enhance the modification effect, thereby enhancing the catalytic activity of the modified resin catalyst.
[0043] In one embodiment, the method comprises: soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then performing the calcination; wherein the soaking temperature can be 10 to 50°C, preferably 20 to 40°C, and the time is 3 to 10 hours, preferably 3 to 5 hours; the calcination temperature can be 70 to 120°C, preferably 90 to 120°C, and the time can be 1 to 5 hours, preferably 2 to 4 hours.
[0044] In this embodiment, the calcination treatment can be performed in an oven to treat the soaked resin. The resin after heat treatment is subsequently treated, and the preferred treatment conditions can make the performance of the modified resin more excellent. By optimizing the heat treatment temperature, the catalytic performance of the modified acidic resin can be further enhanced.
[0045] In one embodiment, the acidic ion exchange resin is selected from a strong acidic ion exchange resin and / or a weak acidic ion exchange resin, preferably a macroporous strong acidic ion exchange resin. In this embodiment, the modified resin obtained by modifying the preferred macroporous strong acidic ion exchange resin has better catalytic performance.
[0046] In one embodiment, the amorphous silicon-aluminum contains 0 to 0.3 wt % of Na 2 O, 50 to 80% by weight of SiO 2 and 20-50 wt% Al 2 O 3 , where Na 2 O、SiO 2 and Al 2 O 3 The content is measured by XRF method; in the XRD spectrum of the amorphous silicon aluminum, only a diffuse diffraction peak appears at 25°~27°, the most probable pore size of the amorphous silicon aluminum is 20~50nm, and x / y is 0.55~0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XRF method.
[0047] In one embodiment, the method for preparing the amorphous silicon-aluminum catalyst comprises: fully mixing a silicon source and an alkali solution at room temperature to 60° C., adding an aluminum source under stirring, adjusting the resulting slurry to an endpoint pH value between 8 and 10.5, and then dynamically aging the slurry at a constant temperature of 40 to 80° C., washing, filtering, and obtaining a solid precipitate; mixing the solid precipitate with a dilute acid solution according to the ratio of solid precipitate: acid: H 2 O=1:(0.02~0.20):(5~30) by weight ratio, contact treatment at room temperature to 60℃ for at least 0.2 hour, filter and dry at 100~150℃; wherein the weight ratio of silicon source to aluminum source is 1:(0.25~1), silicon source is calculated as silicon oxide, and aluminum source is calculated as aluminum oxide; the chemical composition of the amorphous silicon aluminum catalytic material measured by XRF method is: (0~0.3)Na 2 O·(50~80)SiO 2 ·(20~50)Al 2 O 3 ; In the XRD spectrum of the silicon-aluminum material, only a diffuse diffraction peak appears at 25°~27°, and the pore size is between 20~50nm; x / y=0.55~0.75; wherein x represents the Si / Al atomic ratio measured by the XPS method, and y represents the Si / Al atomic ratio measured by the XRF method.
[0048] In one embodiment, the modified acidic resin and amorphous silica-alumina are mechanically mixed to obtain the etherification reaction catalyst.
[0049] In one embodiment, on a dry basis, the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3-3):1, preferably (0.5-2):1, and more preferably (0.7-1.5):1.
[0050] In one embodiment, the average particle size of the modified acidic resin is 350-1250 μm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
[0051] In a second aspect of the present disclosure, an etherification reaction catalyst is prepared by the method described in the first aspect of the present disclosure.
[0052] The third aspect of the present disclosure provides a process for preparing ethylene glycol mono-tert-butyl ether, which comprises: under etherification reaction conditions, contacting ethylene glycol, a C4 olefin raw material containing isobutylene and methyl tert-butyl ether under the catalysis of the etherification reaction catalyst described in the second aspect of the present disclosure.
[0053] In this embodiment, the reaction is performed by loading the etherification reaction catalyst into a reactor selected from a stirred tank reactor, a trickle bed reactor and a fixed bed reactor, preferably a fixed bed reactor, and then adding the reaction materials therein for contact reaction.
[0054] According to the present disclosure, the C4 olefin raw material contains isobutylene. In a preferred embodiment, the mass fraction of isobutylene in the C4 olefin raw material is 5 to 100%, preferably 10 to 100%, so as to further improve the reaction effect of the catalytic etherification reaction.
[0055] In a preferred embodiment, the molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin feedstock to ethylene glycol is 1:1-10, preferably 1:2-4.
[0056] In one embodiment, the etherification reaction conditions include: reaction temperature of 40 to 100°C, preferably 60 to 80°C; reaction pressure of 0.5 to 2.5 MPa, preferably 0.5 to 1.5 MPa; space velocity of 0.1 to 10 h -1 , preferably 0.3~1.0h -1 .
[0057] In the above preferred embodiment, the alcohol-olefin molar ratio of ethylene glycol and the C4 olefin raw material and the conditions of the etherification reaction can act synergistically to further promote the complete reaction, improve the conversion rate of isobutylene and the selectivity of the product ETB, thereby improving the raw material utilization rate and reducing the energy consumption of the subsequent separation process.
[0058] In one embodiment, the method further includes adding an additive to the contact reaction, wherein the additive is selected from water and / or alcohol, preferably one or more of water, ethanol, n-propanol, isopropanol and tert-butanol; based on the total weight of the ethylene glycol and the mixed C4 olefins, the weight of the additive is 0.5 to 20 weight %, preferably 2 to 10 weight %.
[0059] In this embodiment, by adding additives, the acidity of the etherification reaction catalyst can be reduced, the catalyst activity can be adjusted, and further, the generation of by-products can be reduced, and the energy consumption of the product separation step can be reduced; by adjusting the amount of additives, the generation of reaction by-products can also be reduced.
[0060] In one embodiment, the method further includes sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit includes a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.
[0061] In one embodiment, the material obtained by the reaction is separated by the following steps:
[0062] Ethylene glycol 15, C4 olefin raw material 16 and methyl tert-butyl ether 17 are pumped into the etherification reactor 1 for reaction. The bottom material of the etherification reactor 1 enters the C4 removal tower 2, and the mixed C4 material 18 is discharged from the top of the C4 removal tower 2. The bottom material of the C4 removal tower 2 is introduced into the light removal tower 3, and the top material of the light removal tower 3 enters the MTBE removal tower 4. The circulating MTBE 12 discharged from the top of the MTBE removal tower 4 returns to the etherification reactor 1. Methanol 13 is discharged from the bottom of the MTBE removal tower 4 and can be used as a product delivery system. The bottom material of the light removal tower 3 is introduced into the C8 removal tower 5, and the C8 material 19 is discharged from the top of the C8 removal tower 5. The bottom stream of the C8 removal tower 5 enters the azeotropic tower 6, and the top stream of the azeotropic tower 6 enters the ETB separation tower 7. The circulating EDB discharged from the top of the tower 7 11 returns to the etherification reactor 1, ETB product 14 comes out from the bottom of tower 7, the bottom material of azeotropic tower 6 enters ethylene glycol flash tower 8, circulating ethylene glycol 10 comes out from the top of ethylene glycol flash tower 8 and returns to the etherification reactor 1, and heavy component 9 comes out from the bottom of ethylene glycol flash tower 8.
[0063] The present disclosure is further described in detail by way of examples. The raw materials used in the examples can all be obtained through commercial sources.
[0064] Preparation Example 1
[0065] 50g of Amberlyst acidic ion exchange resin (purchased from Tianjin Shuanglian Technology Co., Ltd.) was loaded into a fixed bed reactor, and 100mL of dimethyl sulfone was pumped into the reactor under nitrogen conditions. The acidic ion exchange resin was heated at 80°C for 5h under 5.0MPa conditions, and then the dimethyl sulfone solution was pushed out with nitrogen, and then the solvent was purged with nitrogen. The above resin was placed in a stoppered conical flask, and 200ml of ethanol was added to soak the above resin for 10h, and the ethanol was poured out. The wet resin was roasted in an oven at 105°C for 3h to obtain a modified resin with an average particle size of 600μm.
[0066] The water glass solution (80wt% SiO 2 / L) and a quantitative 1.0M sodium hydroxide solution were fully mixed at room temperature to 60°C, and then Al 2 (SO 4 ) 3 The solution is prepared, the pH value of the obtained slurry is adjusted to be between 8 and 10.5, and then a dynamic aging treatment is performed at a constant temperature of 40 to 80°C, followed by washing and filtering to obtain a solid precipitate; the solid precipitate is mixed with a dilute acid solution according to the ratio of solid precipitate: acid: H 2 O=1:0.15:15 weight ratio, contact treatment at room temperature to 60°C for at least 0.2 hours, filtration and drying at 150°C to obtain amorphous silicon aluminum, which contains 0.3 weight % Na by XRF method. 2 O, 60 wt% SiO 2 and 39.7 wt% Al 2 O 3 In the XRD spectrum, only a diffuse diffraction peak appears at 25°~27°, the most probable pore size is 43nm, the Si / Al atomic ratio x / y measured by the XPS method is 0.65, and the average particle size is 0.050μm.
[0067] The modified resin and the amorphous silicon-alumina were uniformly mixed in a mass ratio of 1.5:1 to obtain an etherification reaction catalyst A1.
[0068] Preparation Example 2
[0069] The preparation method of etherification reaction catalyst A2 is the same as that of Preparation Example 1, except that the heat treatment temperature during the preparation of the modified resin is 110°C.
[0070] Preparation Example 3
[0071] The preparation method of etherification reaction catalyst A3 is the same as that of Preparation Example 1, except that dimethyl sulfone is replaced by an equal volume of cyclobutane sulfone, the heat treatment temperature is 120°C, and the pressure is 3.0 MPa; the heat-treated resin is immersed in ethanol at 30°C for 3h and the calcination temperature is 110°C; and a modified resin catalyst A3 is obtained.
[0072] Preparation Example 4
[0073] The preparation method of etherification reaction catalyst A4 is the same as that of Preparation Example 1, except that the mass ratio of the modified resin to the amorphous silicon aluminum is 1.2:1.
[0074] Preparation Example 5
[0075] The preparation method of etherification reaction catalyst A5 is the same as that of Preparation Example 1, except that the average particle size of the prepared amorphous silicon aluminum is 0.1 μm.
[0076] Preparation Comparative Example 1
[0077] The preparation method of etherification reaction catalyst AZ1 is the same as that of Preparation Example 1, except that the heat treatment temperature during the preparation of the modified resin is 40°C.
[0078] Preparation Comparative Example 2
[0079] The preparation method of etherification reaction catalyst AZ2 is the same as that of Preparation Example 1, except that no dimethyl sulfone is added.
[0080] Preparation Comparative Example 3
[0081] The preparation method of etherification reaction catalyst AZ3 is the same as that of Preparation Example 1, except that no protective gas is used.
[0082] Preparation Comparative Example 4
[0083] The preparation method of the etherification reaction catalyst AZ4 is the same as that of Preparation Example 1, except that the etherification reaction catalyst does not contain amorphous silicon aluminum.
[0084] Preparation Comparative Example 5
[0085] The preparation method of the etherification reaction catalyst AZ5 is the same as that of Preparation Example 1, except that the etherification reaction catalyst does not contain a modified resin.
[0086] Example 1
[0087] 20.0g of catalyst A1 was filled in a fixed bed reactor on a high pressure microreactor test device. Test conditions: 0.20ml / min (12g / h) of ethylene glycol feed, 0.020ml / min (1.2g / h) of water feed, 0.12ml / min (7.2g / h) of C4 olefin feed with a mass fraction of isobutylene of 50%, and 0.055ml / min (2.5g / h) of MTBE were added to the 20mL fixed bed reactor; the molar ratio of olefin to olefin was 1:3, the reaction temperature was 70°C, the reaction pressure was 1.5Mpa, and the space velocity was 1.0h -1 ;
[0088] The mixed material obtained from the fixed bed reactor enters the C4 removal tower, light removal tower, MTBE removal tower, C8 removal tower, azeotropic tower, ETB separation tower and ethylene glycol flash tower for separation in sequence, and ethylene glycol mono-tert-butyl ether product is obtained from the ethylene glycol mono-tert-butyl ether tower. The product properties are listed in Table 1. The olefin molar ratio refers to the molar ratio of the total amount of isobutylene and methyl tert-butyl ether in the C4 olefin raw material to ethylene glycol.
[0089] Example 2
[0090] The process for preparing ETB is the same as that in Example 1, except that the additive is isopropanol, the C4 olefin feed rate is 0.22 ml / min (13.2 g / h), the olefin molar ratio is 1:4, the reaction temperature is 80° C., and the reaction pressure is 1.0 MPa.
[0091] Example 3
[0092] The process for preparing ETB is the same as that in Example 1, except that the mass fraction of isobutylene in the C4 olefin is 5%, and the feed rate of the C4 olefin raw material with a mass fraction of isobutylene of 5% is 0.60 ml / min (36 g / h).
[0093] Example 4
[0094] The process for preparing ETB is the same as that in Example 1, except that no additive water is added.
[0095] Embodiment 5-6
[0096] The process for preparing ETB is the same as that of Example 1, except that catalyst A1 is replaced by equivalent amounts of catalysts A2 and A3, respectively.
[0097] Embodiment 7-8
[0098] The process for preparing ETB is the same as that of Example 1, except that the catalyst Z1 is replaced by equivalent amounts of catalysts A4 and A5, respectively.
[0099] Comparative Examples 1 to 6
[0100] The process for preparing ETB is the same as that of Example 1, except that the catalyst A1 is replaced by equivalent amounts of catalysts AZ1, AZ2, AZ3, AZ4, AZ5 and unmodified Amberlyst acidic ion exchange resin.
[0101] Comparative Example 7
[0102] The process for preparing ETB is the same as that in Example 1, except that MTBE is not added during the preparation process.
[0103] Test Case
[0104] The IB conversion, ETB selectivity, EDB selectivity and isobutylene dimer selectivity were calculated by the following formulas:
[0105] The conversion rate of IB can be accurately determined based on the changes in the amounts of n-butane, isobutane, cis-butene, trans-butene, isobutene and n-butene in the mixed C4.
[0106] IB conversion rate = (1-m IB / m IB0 )×100%, where m IB represents the residual mass of IB in mixed C4, m IB0 Represents the mass of the starting IB in the mixed C4.
[0107] Selectivity of ETB = m ETB / (m ETB +m EDB )×100%;
[0108] Selectivity of EDB = m EDB / (m ETB +m EDB )×100%;
[0109] Among them, m ETB Indicates the mass of ETB, m EDB Indicates the quality of EDB.
[0110] Selectivity of isobutylene dimer = m DIB / (m DIB +m IB )×100%. Among them, m DIB Indicates the mass of isobutylene dimer, m IB represents the residual mass of IB.
[0111] See Table 1 for detailed data.
[0112] Table 1
[0113]
[0114]
[0115] According to the data analysis in Table 1, it can be seen from the data of Examples 1 to 8 and Comparative Examples 1 to 7 that the use of the modified resin prepared by the present invention for etherification reaction can enhance the IB conversion rate and the selectivity of ETB, and reduce the selectivity of EDB and the selectivity of isobutylene dimer; it can be seen from the data of Example 3 that when the mass fraction of isobutylene in the reaction raw material C4 olefin is as low as 5%, the etherification reaction effect using the modified acidic resin catalyst of the present application is also good; compared with the data of Example 1 and Example 4, it can be seen that in the preferred embodiment of the present application in which additives are added during the etherification reaction, the content of reaction by-products can be further reduced; compared with the data of Example 1 and Example 5, it can be seen that in the preferred heat treatment temperature range of 100 to 130° C. in the present application, the etherification reaction effect is better. By comparing the data in Example 1 and Examples 7-8, it can be seen that in the embodiment in which the preferred etherification reaction catalyst of the present invention contains amorphous silica-alumina, and the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3 to 3): 1. The average particle size of the modified acidic resin is 0.350 to 1.250 mm, and the average particle size of the amorphous silica-alumina is 0.030 to 0.100 μm, the reaction effect of the etherification reaction can be better.
[0116] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0117] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0118] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing an etherification reaction catalyst, It is characterized in that The etherification reaction catalyst comprises a mixture of modified resin and amorphous silicon-aluminum; The method comprises preparing the modified resin by the following steps: Under protective atmosphere conditions, the organic sulfone and the acidic ion exchange resin are contacted at 50 to 200° C. for heat treatment, and the liquid material is separated and removed from the obtained mixed material to obtain a heat-treated resin; the heat-treated resin is contacted with an organic solvent and then calcined to obtain a modified resin; The organic sulfone has 2 to 10 carbon atoms; The calcination temperature is 70-120°C; The amorphous silicon aluminum contains 0 to 0.3 wt % of Na 2 O, 50 to 80% by weight of SiO 2 and 20-50 wt% Al 2 O 3 , where Na 2 O、SiO 2 and Al 2 O 3 The content was measured by XRF method; In the XRD spectrum of the amorphous silicon aluminum, only a diffuse diffraction peak appears at 25°~27°, the most probable pore size of the amorphous silicon aluminum is 20~50nm, and x / y is 0.55~0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by the XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by the XRF method.
2. The method according to claim 1, It is characterized in that The organic sulfone is selected from one or more of dimethyl sulfone, methyl vinyl sulfone, cyclobutene sulfone, cyclopentane sulfone, diethyl sulfone and allyl sulfone.
3. The method according to claim 2, It is characterized in that The organic sulfone is selected from one or more of dimethyl sulfone, cyclobutane sulfone and allyl sulfone.
4. The method according to claim 1, It is characterized in that The protective atmosphere is selected from one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide.
5. The method according to claim 4, It is characterized in that The protective atmosphere is selected from nitrogen.
6. The method according to claim 1, It is characterized in that The heat treatment conditions include a pressure of 0.1 to 20.0 MPa, a temperature of 80 to 150° C., and a time of 0.5 to 20 h; relative to 1 g of the acidic ion exchange resin, the amount of the organic sulfone is 0.5 to 2.5 mL.
7. The method according to claim 1, It is characterized in that The organic solvent includes one or more of ethanol, n-propanol, n-butanol, isopropanol, isobutanol, sec-butanol and tert-butanol.
8. The method according to claim 7, It is characterized in that The organic solvent includes ethanol.
9. The method according to claim 1, It is characterized in that The method comprises: soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then calcining; the soaking temperature is 10-50°C, the time is 3-10 hours; the calcining time is 1-5 hours.
10. The method according to claim 1, It is characterized in that The acidic ion exchange resin is selected from a strongly acidic ion exchange resin and / or a weakly acidic ion exchange resin.
11. The method according to claim 10, It is characterized in that The acidic ion exchange resin is selected from macroporous strongly acidic ion exchange resin.
12. The method according to claim 1, It is characterized in that The method further comprises mixing the modified resin and the amorphous silica-alumina to obtain the etherification reaction catalyst.
13. The method according to claim 1, It is characterized in that Calculated on a dry basis, the mass ratio of the modified resin to the amorphous silicon-aluminum is (0.3-3):
1.
14. The method according to claim 1, It is characterized in that The average particle size of the modified resin is 350-1250 μm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
15. An etherification reaction catalyst prepared by the method according to any one of claims 1 to 14.
16. A process for preparing ethylene glycol mono-tert-butyl ether, It is characterized in that The process comprises: under etherification reaction conditions, ethylene glycol, C4 olefin raw material containing isobutylene and methyl tert-butyl ether are contacted and reacted under the catalysis of the etherification reaction catalyst described in claim 15.
17. The process according to claim 16, It is characterized in that The mass fraction of isobutylene in the C4 olefin raw material is 5 to 100%; The molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin raw material to the ethylene glycol is 1:1-10.
18. The process according to claim 17, It is characterized in that The mass fraction of isobutylene in the C4 olefin raw material is 10-100%.
19. The process according to claim 17, It is characterized in that The molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin raw material to the ethylene glycol is 1:2-4.
20. The process according to claim 16, It is characterized in that The method further comprises adding an additive to the contact reaction, wherein the additive is water and / or alcohol; Based on the total weight of the ethylene glycol and the mixed C4 olefins, the weight of the additive is 0.5 to 20 weight %.
21. The process according to claim 20, It is characterized in that The additive is one or more of water, ethanol, n-propanol, isopropanol and tert-butanol.
22. The process according to claim 20, It is characterized in that Based on the total weight of the ethylene glycol and the mixed C4 olefins, the weight of the additive is 2 to 10 weight %.
23. The process according to claim 16, It is characterized in that The etherification reaction conditions include: reaction temperature of 40-100°C, reaction pressure of 0.5-2.5 MPa, space velocity of 0.1-10 h -1 .
24. The process according to claim 23, It is characterized in that The reaction temperature is 60-80°C.
25. The process according to claim 23, It is characterized in that The reaction pressure is 0.5~1.5MPa.
26. The process according to claim 23, It is characterized in that Airspeed: 0.3~1.0h -1 .
27. The process according to claim 16, It is characterized in that The method also includes sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit includes a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.